Polybutadiene organic silicon dihydric alcohol, preparation method thereof and thermoplastic organic silicon polyurethane elastomer

Through the combination of polybutadiene silicone diol and diisocyanate and other materials, the shortcomings of thermoplastic polyurethane elastomers in low temperature resistance and surface inertia are solved, and the transparency and mechanical properties are improved, which are suitable for a variety of applications field.

CN118930873AActive Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411201146.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing thermoplastic polyurethane elastomers have shortcomings in low temperature resistance and surface inertia, especially in the fields of transparent TPU films and shoe materials. The introduction of silicones will lead to phase separation and reduced transparency, limiting their application.

Method used

Using polybutadiene silicone diol as raw material, the thermoplastic silicone polyurethane elastomer with moderate solubility parameters is prepared by polycondensation reaction of end carboxylic polybutadiene and end hydroxyl polydimethylsiloxane. Diisocyanate, other diols and chain extenders form Si-TPU with excellent mechanical properties and transparency.

Benefits of technology

It realizes the Si-TPU's transparency, excellent mechanical properties, low temperature resilience and surface hydrophobicity. It is suitable for applications in medical supplies, clothing, protective supplies and other fields, and the preparation method is simple and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017879060000031
    Figure BDA0005017879060000031
  • Figure BDA0005017879060000032
    Figure BDA0005017879060000032
  • Figure BDA0005017879060000041
    Figure BDA0005017879060000041
Patent Text Reader

Abstract

The invention relates to the field of polyurethane elastomer materials, in particular to polybutadiene organic silicon dihydric alcohol, a preparation method of the polybutadiene organic silicon dihydric alcohol and a thermoplastic organic silicon polyurethane elastomer. According to the present invention, the phase separation degree of the thermoplastic organic silicon polyurethane elastomer contained in the molecular chain of the prepared thermoplastic organic silicon polyurethane elastomer is low, the product has unexpected good transparency, and the elastomer has characteristics of PDMS and CTPB, and has characteristics of excellent mechanical property, outstanding low-temperature resilience, outstanding aging resistance, excellent surface hydrophobicity, excellent smoothness and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyurethane elastomer materials, and in particular to a polybutadiene organosilicon diol and a preparation method thereof, and a thermoplastic organosilicon polyurethane elastomer. Background Art

[0002] Thermoplastic polyurethane elastomer (TPU) is a polymer synthetic material with excellent comprehensive performance. It has excellent mechanical properties of high strength, high elasticity, high wear resistance and high flexibility. It is also resistant to oil, solvents and chemicals. There are many varieties of TPU materials such as films, pipes, shoe materials, wires, cables, sheets, etc., so it can be widely used in various fields.

[0003] Although TPU has many excellent properties, its low temperature resistance and surface inertness are not satisfactory. Many scholars have conducted research on this. Polydimethylsiloxane (PDMS) in the silicone series products has excellent flexibility, and its Tg is less than -100°C. In addition, it has extremely low surface energy and is prone to surface migration. Therefore, some scholars use PDMS to synthesize and modify TPU to improve the low temperature resistance and surface inertness of TPU.

[0004] Patent CN 106565933A discloses a method for preparing silicone thermoplastic polyurethane. The invention uses polyester / polyether polyol, reactive PDMS at both ends, chain extender, and diisocyanate as raw materials, and prepares a silicon-containing TPU (Si-TPU) material with a PDMS structure in the main molecular chain through different feeding orders. Patent CN109485826A uses single-end mono / bifunctional reactive silicone as raw materials to prepare a Si-TPU with silicone segments distributed at the ends / side chains of the product molecules. The silicone segments at the ends / side chains are more likely to migrate to the surface than the silicone segments in the chain, so that the Si-TPU elastomer has good surface hydrophobicity and low temperature resistance. Patent US 006313254B1 discloses the preparation, composition and properties of a polyurethane elastomer containing polysiloxane. The invention uses MDI / BDO as the hard segment, and at least one polysiloxane macromolecular diol and at least one polyether / polycarbonate macromolecular diol as the soft segment to prepare a Si-TPU product containing PDMS in the main molecular chain. Patent CN104448231A uses polyether silicone block polymer PEO-PDMS-PEO as raw material to prepare a Si-TPU elastomer with good mechanical properties, low temperature resistance and surface hydrophobicity.

[0005] In the field of transparent TPU films, there are very high requirements for transparency and surface mucosa, i.e. surface inertness; for example, the air cushion material on shoes also has very high requirements for transparency and low-temperature resilience, i.e. low-temperature resistance. Although the above methods can effectively improve the low-temperature resistance and surface inertness of TPU, due to the extremely low solubility parameter and high incompatibility of silicone, it is easy to cause serious phase separation of the product. Introducing silicone into the TPU molecular chain will make the product completely opaque or have a very low transmittance, thus limiting the application of this type of Si-TPU. Currently, there are few reports on the preparation of transparent Si-TPU. Summary of the invention

[0006] Therefore, the object of the present invention is to provide a polybutadiene silicone diol and a preparation method thereof and a thermoplastic silicone polyurethane elastomer. The polybutadiene silicone diol of formula (I) has a moderate solubility parameter, and the Si-TPU prepared therefrom has a small degree of phase separation and good product transparency. The elastomer has the characteristics of polydimethylsiloxane (PDMS) and carboxyl-terminated polybutadiene (CTPB), and also has excellent mechanical properties, outstanding low-temperature resilience, surface hydrophobicity and smoothness.

[0007] In order to achieve the above invention object, the technical solution provided by the present invention is as follows:

[0008] A polybutadiene organosilicon diol, the structural formula of which is shown in formula (I):

[0009]

[0010] Wherein, m is an integer of 1-23, x is an integer of 1-17, y is an integer of 1-8, n is an integer of 2-12, R 1 It is one of an alkyl group, an ether group, and an ester group containing 1 to 8 carbon atoms.

[0011] Further, m is an integer of 2-15; and / or, x is an integer of 2-9; and / or, y is an integer of 2-6; and / or, n is an integer of 4-10.

[0012] Furthermore, R 1 -CH 2 -、-CH 2 CH 2 -、-CH 2 CH 2 CH 2 -、#-CH 2 OCH 2 CH 2 -*、-CH 2 CH 2 OCH 2 CH2 -、*-CH 2 CH 2 OCH 2 CH 2 CH 2 -#、#-CH 2 COOCH 2 CH 2 -* or #-CH 2 CH 2 CH 2 COOCH 2 CH 2 CH 2 CH 2 -*, where the * end is connected to the oxygen atom and the # end is connected to the silicon atom.

[0013] Furthermore, the polybutadiene silicone diol has a hydroxyl value of 5.3-29.1 mgKOH / g and an acid value of 0.01-0.5 mgKOH / g.

[0014] On the other hand, the present invention provides a method for preparing a polybutadiene organosilicon diol, comprising the following steps: mixing carboxyl-terminated polybutadiene and hydroxyl-terminated polydimethylsiloxane, and subjecting the mixture to polycondensation to obtain the polybutadiene organosilicon diol, wherein the carboxyl-terminated polybutadiene has a structural formula as shown in formula (II), and the hydroxyl-terminated polydimethylsiloxane has a structural formula as shown in formula (III).

[0015]

[0016]

[0017] Wherein, m, x, and y in formula (II) and formula (III) are the same as defined above, and R in formula (III) is 1 As defined above.

[0018] Furthermore, the molar ratio of the terminal hydroxyl polydimethylsiloxane to the terminal carboxyl polybutadiene is 1 to 2.5:1; and / or, during the polycondensation reaction, the system is first heated to 140-230° C. under the protection of an inert gas for reaction for 2-6 hours, then continuously heated to 210-280° C. for reaction for 2-8 hours, and then the vacuum system is turned on to continue the reaction under vacuum conditions (until the hydroxyl value and acid value are qualified).

[0019] On the other hand, the present invention also provides a thermoplastic organosilicon polyurethane elastomer, the raw materials for its preparation include the polybutadiene organosilicon diol or the polybutadiene organosilicon diol prepared by the preparation method; preferably, based on 100 parts by weight of the total weight of the raw materials, the raw materials for the preparation of the thermoplastic organosilicon polyurethane elastomer include the following components:

[0020] (1) diisocyanate: 19 to 42 parts, preferably 28 to 38 parts;

[0021] (2) the polybutadiene silicone diol: 28 to 57 parts, preferably 34 to 47 parts;

[0022] (3) other diols: 6 to 44 parts, preferably 15 to 27 parts;

[0023] (4) Chain extender: 4 to 15 parts, preferably 5 to 9 parts.

[0024] Furthermore, the thermoplastic silicone polyurethane elastomer also satisfies at least one of the following (1)-(4):

[0025] (1) The diisocyanate is one or more of aliphatic, alicyclic and aromatic diisocyanates; preferably at least one of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, p-phenylene diisocyanate, naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, xylylene diisocyanate, cyclohexane dimethylene diisocyanate, trimethyl-1,6-hexamethylene diisocyanate, tetramethyl meta-xylylene diisocyanate, norbornane diisocyanate, dimethyl biphenyl diisocyanate, methylcyclohexyl diisocyanate, dimethyl diphenylmethane diisocyanate and lysine diisocyanate;

[0026] (2) the number average molecular weight of the other diol is 800-8000 g / mol, preferably 1000-6000 g / mol;

[0027] (3) The other diols are other macromolecular diols having two terminal hydroxyl groups; preferably, the other diols are one or more of aliphatic or aromatic polyester diols, aliphatic or aromatic polyether diols, aliphatic or aromatic polycarbonate diols, aliphatic or aromatic polylactic acid diols, and aliphatic or aromatic polyolefin diols; more preferably, the other diols are one or more of polytetrahydrofuran diol, polybutylene adipate diol, polycarbonate diol, poly(1,6-hexanediol terephthalate) diol, polyoxypropylene diol, and polyethylene adipate diol;

[0028] (4) The chain extender is a small molecule chain extender, preferably an aliphatic and / or aromatic small molecule chain extender; more preferably ethylene glycol, 1,4-butanediol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, neopentyl glycol, methyl propylene glycol, 1,6-hexanediol, 1,3-propylene glycol, dipropylene glycol, tripropylene glycol, butyl ethyl propylene glycol, diethyl pentanediol, 3-methyl-1,5-pentanediol, 1,3-butanediol, 1,2-butanediol, 2,3-butanediol, trimethyl pentanediol, 1,5-pentanediol, 1,2-pentanediol, hydroxy neopentyl glycol, 1,6-hexanediol, 1,3-propanediol ... One or more of hydroxyneopentyl valerate, 2-ethyl-1,3-hexanediol, dodecanediol, 1,4-dihydroxymethylcyclohexane, 1,4-cyclohexanediol, hydroquinone dihydroxyethyl ether, resorcinol dihydroxyethyl ether, resorcinol bishydroxypropyl ether, resorcinol bishydroxypropyl ethyl ether, 4-hydroxyethyloxyethyl-1-hydroxyethylphenylene diether, 3-hydroxyethyloxyethyl-1-hydroxyethylphenylene diether, bisphenol A dihydroxyethyl ether, bisphenol A dihydroxypropyl ether, 1,4-cyclohexanediamine, diaminodicyclohexylmethane, trimethylhexanediamine, and dimethyldiaminodicyclohexylmethane.

[0029] In some more preferred embodiments, the diisocyanate is one or more of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate and p-phenylene diisocyanate.

[0030] In some more preferred embodiments, the other diols are one or more of polytetramethylene glycol, polybutylene adipate glycol, polycarbonate glycol, polyhexane terephthalate glycol, and polyoxypropylene glycol.

[0031] In some more preferred embodiments, the chain extender is one or more of ethylene glycol, 1,4-butanediol, diethylene glycol, 1,6-hexanediol, 1,3-propylene glycol, dipropylene glycol, 1,5-pentanediol, and 1,4-cyclohexanediamine.

[0032] On the other hand, the present invention also provides a method for preparing the thermoplastic silicone polyurethane elastomer, comprising the following steps:

[0033] The polybutadiene silicone diol, other diols and a chain extender are mixed to obtain a mixture; the mixture is mixed with diisocyanate to react to obtain a thermoplastic silicone polyurethane elastomer;

[0034] Optionally, the reaction temperature is 80-160°C.

[0035] On the other hand, the present invention provides the use of the above-mentioned thermoplastic silicone polyurethane elastomer or the thermoplastic silicone polyurethane elastomer prepared by the preparation method in medical supplies, clothing supplies, protective supplies, smart wearable devices, cables, and automotive supplies, such as for the surface of luggage, electronic product sheaths, medical devices, wires and cables, car seats, etc.

[0036] The technical solution of the present invention has the following advantages:

[0037] 1. The polybutadiene silicone diol provided by the present invention, the polybutadiene silicone diol of the structure of formula (I) has a moderate solubility parameter, and the thermoplastic silicone polyurethane elastomer prepared therefrom has a small degree of phase separation of the elastomer contained in the molecular chain, and the product has unexpectedly good transparency. In addition, the elastomer has the characteristics of both PDMS and CTPB. Therefore, the thermoplastic silicone polyurethane elastomer prepared by the present invention has not only good transparency, but also excellent mechanical properties, outstanding low-temperature resilience, aging resistance, surface hydrophobicity and smoothness.

[0038] 2. The preparation method of the polybutadiene organosilicon diol provided by the present invention is simple, easy to operate, and suitable for industrial production. The polybutadiene organosilicon diol is obtained by polycondensation reaction of carboxyl-terminated polybutadiene and hydroxyl-terminated polydimethylsiloxane, and during the reaction, the carboxyl group of the carboxyl-terminated polybutadiene and the hydroxyl group of the hydroxyl-terminated polydimethylsiloxane undergo esterification reaction.

[0039] 3. The thermoplastic silicone polyurethane elastomer provided by the present invention is prepared by using polybutadiene silicone diol of formula (I) as a raw material. The prepared elastomer has significantly improved transparency and has the characteristics of both PDMS and CTPB. It also has excellent mechanical properties, outstanding low-temperature resilience, surface hydrophobicity and smoothness.

[0040] By controlling the value of m, x, y or n in the structure of formula (I) within the preferred range or R 1 The comprehensive properties of the prepared elastomer can be further improved by controlling the weight fractions of polybutadiene silicone diol, other diols, chain extenders, and diisocyanates within the preferred range and the types of these substances within the preferred range. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0043] Example 1

[0044] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps:

[0045] Carboxyl-terminated polybutadiene (CTPB) (x is 8, y is 3), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 -CH 2 CH 2 CH 2 -, m is 10) was added into the reaction kettle at a molar ratio of PDMS-OH / CTPB of 1.5:1, and under the protection of inert gas, the system was heated to 180°C for reaction for 4 hours, then continuously heated to 250°C for reaction for 5 hours, and then the vacuum system was turned on, and the reaction was continued under vacuum conditions until the hydroxyl value and acid value were qualified, and the temperature was lowered and the material was discharged to obtain polybutadiene silicone diol. The hydroxyl value was 14.9 mgKOH / g, and the acid value was 0.05 mgKOH / g.

[0046] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0047]

[0048] Where m is 10, x is 8, y is 3, R 1 -CH 2 CH 2 CH 2 -.

[0049] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0050] (1) Diisocyanate: diphenylmethane diisocyanate, 32 parts;

[0051] (2) 38 parts of polybutadiene organosilicon diol prepared in this example;

[0052] (3) Other macromolecular diols: polytetrahydrofuran diol, number average molecular weight 2000 g / mol, 22 parts;

[0053] (4) Small molecule chain extender: 1,4-butanediol, 8 parts.

[0054] The preparation method comprises the following steps:

[0055] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0056] 2) adding diisocyanate to the mixture of step 1), reacting at 100° C. for 2 minutes to obtain a thermoplastic polyurethane elastomer.

[0057] Example 2

[0058] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps:

[0059] Carboxyl-terminated polybutadiene (CTPB) (x is 17, y is 8), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 For *-CH 2 CH 2 OCH 2 CH 2 CH 2 -#, where the * end is connected to the oxygen atom, the # is connected to the silicon atom, and m is 15) was added to the reactor at a molar ratio of PDMS-OH / CTPB of 1.2:1. Under the protection of inert gas, the system was heated to 140°C for reaction for 6 hours, then continuously heated to 210°C for reaction for 8 hours, and then the vacuum system was turned on. The reaction continued under vacuum conditions until the hydroxyl value and acid value were qualified, and the temperature was lowered to obtain polybutadiene silicone diol. The hydroxyl value of polybutadiene silicone diol was 11.2 mgKOH / g, and the acid value was 0.01 mgKOH / g.

[0060] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0061]

[0062] Among them, m is 15, x is 17, y is 8, R 1 For *-CH 2 CH 2 OCH 2 CH 2 CH 2 -#, where the * end is connected to the oxygen atom and the # end is connected to the silicon atom.

[0063] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0064] (1) Diisocyanate: hexamethylene diisocyanate, 25 parts;

[0065] (2) 47 parts of polybutadiene silicone diol prepared in this example;

[0066] (3) Other macromolecular diols: polytetrahydrofuran diol, number average molecular weight 8000 g / mol, 23 parts;

[0067] (4) Small molecule chain extender: 1,6-hexanediol, 5 parts.

[0068] The preparation method comprises the following steps:

[0069] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0070] 2) adding diisocyanate to the mixture of step 1), reacting at 120° C. for 2 min to obtain a thermoplastic polyurethane elastomer.

[0071] Example 3

[0072] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps: treating carboxyl-terminated polybutadiene (CTPB) (x is 2, y is 1), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 For #-CH 2 CH 2 CH 2 COOCH 2 CH 2 CH 2 CH 2 -*, where the * end is connected to the oxygen atom, # is connected to the silicon atom, and m is 2) was added into the reactor at a molar ratio of PDMS-OH / CTPB of 2:1, and the system was heated to 230°C for reaction for 2h under the protection of inert gas, and then the temperature was continuously raised to 280°C for further reaction for 2h, and then the vacuum system was turned on, and the reaction was continued under vacuum conditions until the hydroxyl value and acid value were qualified, and the temperature was lowered and the material was discharged to obtain polybutadiene silicone diol. The hydroxyl value of polybutadiene silicone diol was 29.1mgKOH / g, and the acid value was 0.31mgKOH / g.

[0073] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0074]

[0075] Where m is 2, x is 2, y is 1, and R 1 For #-CH 2 CH 2 CH 2 COOCH 2 CH2 CH 2 CH 2 -*, where the * end is connected to the oxygen atom and the # end is connected to the silicon atom.

[0076] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0077] (1) Diisocyanate: xylylene diisocyanate, 42 parts;

[0078] (2) 28 parts of polybutadiene organosilicon diol prepared in this example;

[0079] (3) Other macromolecular diols: polybutylene adipate diol, number average molecular weight 1000 g / mol, 15 parts;

[0080] (4) Small molecule chain extender: 1,4-butanediol, 15 parts.

[0081] The preparation method comprises the following steps:

[0082] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0083] 2) adding diisocyanate to the mixture of step 1), reacting at 80° C. for 1 min to obtain a thermoplastic polyurethane elastomer.

[0084] Example 4

[0085] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps: treating carboxyl-terminated polybutadiene (CTPB) (x is 14, y is 9), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 -CH 2 -, m is 23) was added into the reactor at a molar ratio of PDMS-OH / CTPB of 1:1, and under the protection of inert gas, the system was heated to 160°C for reaction for 3 hours, then continuously heated to 230°C for reaction for 4 hours, and then the vacuum system was turned on, and the reaction was continued under vacuum conditions until the hydroxyl value and acid value were qualified, and the temperature was lowered and the material was discharged to obtain polybutadiene silicone diol. The hydroxyl value was 5.3 mgKOH / g, and the acid value was 0.35 mgKOH / g.

[0086] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0087]

[0088] Among them, m is 23, x is 14, y is 9, R1 -CH 2 -.

[0089] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0090] (1) Diisocyanate: p-phenylene diisocyanate, 19 parts;

[0091] (2) 52 parts of polybutadiene organosilicon diol prepared in this example;

[0092] (3) Other macromolecular diols: polycarbonate diol, number average molecular weight 2000 g / mol, 24 parts;

[0093] (4) Small molecule chain extender: dipropylene glycol, 5 parts.

[0094] The preparation method comprises the following steps:

[0095] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0096] 2) adding diisocyanate to the mixture of step 1), reacting at 160° C. for 1 min to obtain a thermoplastic polyurethane elastomer.

[0097] Example 5

[0098] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps: treating carboxyl-terminated polybutadiene (CTPB) (x is 9, y is 6), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 -CH 2 CH 2 -, m is 6) was added into the reaction kettle at a molar ratio of PDMS-OH / CTPB of 2.5:1, and the system was heated to 200°C for reaction for 5 hours under the protection of inert gas, and then the temperature was continuously raised to 250°C for reaction for 6 hours, and then the vacuum system was turned on, and the reaction was continued under vacuum conditions until the hydroxyl value and acid value were qualified, and the temperature was lowered and the material was discharged to obtain polybutadiene silicone diol. The hydroxyl value was 7mgKOH / g, and the acid value was 0.5mgKOH / g.

[0099] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0100]

[0101] Among them, m is 6, x is 9, y is 6, R 1 -CH 2 CH2 -.

[0102] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0103] (1) Diisocyanate: isophorone diisocyanate, 38 parts;

[0104] (2) 44 parts of polybutadiene organosilicon diol prepared in this example;

[0105] (3) Other macromolecular diols: poly(1,6-hexanediol terephthalate), number average molecular weight 6000 g / mol, 9 parts;

[0106] (4) Small molecule chain extender: hydroquinone dihydroxyethyl ether, 9 parts.

[0107] The preparation method comprises the following steps:

[0108] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0109] 2) adding diisocyanate to the mixture of step 1), reacting at 90° C. for 2 min to obtain a thermoplastic polyurethane elastomer.

[0110] Example 6

[0111] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps: treating carboxyl-terminated polybutadiene (CTPB) (x is 3, y is 2), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 For #-CH 2 COOCH 2 CH 2 -*, where the * end is connected to the oxygen atom, the # is connected to the silicon atom, and m is 5) was added into the reactor at a molar ratio of PDMS-OH / CTPB of 1.8:1, and the system was heated to 150°C for 4 hours under the protection of inert gas, and then the temperature was continuously raised to 220°C for 5 hours, and then the vacuum system was turned on, and the reaction was continued under vacuum conditions until the hydroxyl value and acid value were qualified, and the temperature was lowered to obtain polybutadiene silicone diol. The hydroxyl value was 23.2 mgKOH / g, and the acid value was 0.22 mgKOH / g.

[0112] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0113]

[0114] Where m is 5, x is 3, y is 2, R 1 For #-CH 2 COOCH 2 CH 2 -*, where the * end is connected to the oxygen atom and the # end is connected to the silicon atom.

[0115] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0116] (1) Diisocyanate: cyclohexane dimethylene diisocyanate, 24 parts;

[0117] (2) 34 parts of polybutadiene organosilicon diol prepared in this example;

[0118] (3) Other macromolecular diols: polyethylene adipate diol, number average molecular weight 3000 g / mol, 38 parts;

[0119] (4) Small molecule chain extender: 1,4-cyclohexanediol, 4 parts.

[0120] The preparation method comprises the following steps:

[0121] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0122] 2) adding diisocyanate to the mixture of step 1), reacting at 120° C. for 2 min to obtain a thermoplastic polyurethane elastomer.

[0123] Example 7

[0124] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps: treating carboxyl-terminated polybutadiene (CTPB) (x is 1, y is 4), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 -CH 2 CH 2 OCH 2 CH 2 -, m is 12) was added into the reaction kettle at a molar ratio of PDMS-OH / CTPB of 1.4:1, and under the protection of inert gas, the system was heated to 190°C for reaction for 3 hours, then continuously heated to 240°C for reaction for 6 hours, and then the vacuum system was turned on, and the reaction was continued under vacuum conditions until the hydroxyl value and acid value were qualified, and the temperature was lowered and the material was discharged to obtain polybutadiene silicone diol. The hydroxyl value was 8.4 mgKOH / g, and the acid value was 0.27 mgKOH / g.

[0125] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0126]

[0127] Where m is 12, x is 1, y is 4, R 1 -CH 2 CH 2 OCH 2 CH 2 -.

[0128] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0129] (1) Diisocyanate: toluene diisocyanate, 20 parts;

[0130] (2) 29 parts of polybutadiene organosilicon diol prepared in this example;

[0131] (3) Other macromolecular diols: polyoxypropylene glycol, number average molecular weight 5000 g / mol, 44 parts;

[0132] (4) Small molecule chain extender: 1,3-propylene glycol, 7 parts.

[0133] The preparation method comprises the following steps:

[0134] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0135] 2) adding diisocyanate to the mixture of step 1), reacting at 130° C. for 2 minutes to obtain a thermoplastic polyurethane elastomer.

[0136] Example 8

[0137] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps: treating carboxyl-terminated polybutadiene (CTPB) (x is 2, y is 1), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 For #-CH 2 OCH 2 CH 2-*, where the * end is connected to the oxygen atom, the # is connected to the silicon atom, and m is 1) is added into the reactor at a molar ratio of PDMS-OH / CTPB of 1.5:1, and the system is heated to 170°C for reaction for 5 hours under the protection of an inert gas such as nitrogen, and then the temperature is continuously raised to 230°C for reaction for 4 hours, and then the vacuum system is turned on, and the reaction is continued under vacuum conditions until the hydroxyl value and acid value are qualified, and the temperature is lowered and the material is discharged to obtain polybutadiene silicone diol. The hydroxyl value is 15.5 mgKOH / g, and the acid value is 0.38 mgKOH / g.

[0138] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0139]

[0140] Where m is 1, x is 2, y is 1, R 1 For #-CH 2 OCH 2 CH 2 -*, where the * end is connected to the oxygen atom and the # end is connected to the silicon atom.

[0141] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0142] (1) Diisocyanate: xylylene diisocyanate, 28 parts;

[0143] (2) 57 parts of polybutadiene organosilicon diol prepared in this example;

[0144] (3) Other macromolecular diols: polyethylene adipate diol, number average molecular weight 800 g / mol, 6 parts;

[0145] (4) Small molecule chain extender: tripropylene glycol, 9 parts.

[0146] The preparation method comprises the following steps:

[0147] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0148] 2) adding diisocyanate to the mixture of step 1), reacting at 120° C. for 3 minutes to obtain a thermoplastic polyurethane elastomer.

[0149] Example 9

[0150] This embodiment provides a method for preparing polybutadiene organosilicon diol, comprising the following steps: treating carboxyl-terminated polybutadiene (CTPB) (x is 6, y is 4), hydroxy-terminated polydimethylsiloxane (PDMS-OH) (R 1 -CH 2 CH 2 CH 2 -, m is 8) was added into the reaction kettle at a molar ratio of PDMS-OH / CTPB of 1.6:1, and under the protection of inert gas, the system was heated to 180°C for reaction for 3 hours, then continuously heated to 240°C for reaction for 5 hours, and then the vacuum system was turned on, and the reaction was continued under vacuum conditions until the hydroxyl value and acid value were qualified, and the temperature was lowered and the material was discharged to obtain polybutadiene silicone diol. The hydroxyl value was 14 mgKOH / g, and the acid value was 0.06 mgKOH / g.

[0151] The structural formula of the prepared polybutadiene silicone diol is as follows:

[0152]

[0153] Among them, m is 8, x is 6, y is 4, R 1 -CH 2 CH 2 CH 2 -.

[0154] This embodiment provides a thermoplastic silicone polyurethane elastomer, and the raw materials thereof, calculated based on 100 parts by total weight, include:

[0155] (1) Diisocyanate: diphenylmethane diisocyanate, 31 parts;

[0156] (2) 35 parts of polybutadiene organosilicon diol prepared in this example;

[0157] (3) Other macromolecular diols: polytetrahydrofuran diol, number average molecular weight 2000 g / mol, 27 parts;

[0158] (4) Small molecule chain extender: ethylene glycol, 7 parts.

[0159] The preparation method comprises the following steps:

[0160] 1) uniformly mixing polybutadiene silicone diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0161] 2) adding diisocyanate to the mixture of step 1), reacting at 100° C. for 2 minutes to obtain a thermoplastic polyurethane elastomer.

[0162] Comparative Example 1

[0163] This comparative example provides a thermoplastic silicone polyurethane elastomer, and its raw materials, calculated on a total weight basis of 100 parts, include:

[0164] (1) Diisocyanate: diphenylmethane diisocyanate, 32 parts;

[0165] (2) Polybutadiene diol: 38 parts, purchased from Lanzhou Petrochemical Company, with the structural formula (x 1 is 22, y 1 is 12);

[0166] (3) Other macromolecular diols: polytetrahydrofuran diol, number average molecular weight 2000 g / mol, 22 parts;

[0167] (4) Small molecule chain extender: 1,4-butanediol, 8 parts.

[0168] The preparation method comprises the following steps:

[0169] 1) mixing polybutadiene diol, other macromolecular diols and small molecular chain extenders uniformly to obtain a mixture;

[0170] 2) adding diisocyanate to the mixture of step 1), reacting at 100° C. for 2 minutes to obtain a thermoplastic butadiene polyurethane elastomer.

[0171] Comparative Example 2

[0172] This comparative example provides a thermoplastic silicone polyurethane elastomer, and its raw materials, calculated on a total weight basis of 100 parts, include:

[0173] (1) Diisocyanate: diphenylmethane diisocyanate, 32 parts;

[0174] (2) Polydimethylsiloxane diol: 38 parts, purchased from WACKER Company, with the structural formula (m 1 is 24);

[0175] (3) Other macromolecular diols: polytetrahydrofuran diol, number average molecular weight 2000 g / mol, 22 parts;

[0176] (4) Small molecule chain extender: 1,4-butanediol, 8 parts.

[0177] The preparation method comprises the following steps:

[0178] 1) uniformly mixing polydimethylsiloxane diol, other macromolecular diols, and small molecular chain extenders to obtain a mixture;

[0179] 2) adding diisocyanate to the mixture of step 1), reacting at 100° C. for 2 min to obtain a thermoplastic silicone polyurethane elastomer.

[0180] Comparative Example 3

[0181] This comparative example provides a thermoplastic silicone polyurethane elastomer, and its raw materials, calculated on a total weight basis of 100 parts, include:

[0182] (1) Diisocyanate: diphenylmethane diisocyanate, 32 parts;

[0183] (2) Other macromolecular diols: polytetrahydrofuran diol, number average molecular weight 2000 g / mol, 60 parts;

[0184] (4) Small molecule chain extender: 1,4-butanediol, 8 parts.

[0185] The preparation method comprises the following steps:

[0186] 1) mixing other macromolecular diols and small molecular chain extenders uniformly to obtain a mixture;

[0187] 2) adding diisocyanate to the mixture of step 1), reacting at 100° C. for 2 minutes to obtain a thermoplastic polyurethane elastomer.

[0188] Comparative Example 4

[0189] This comparative example provides a thermoplastic silicone polyurethane elastomer, and its raw materials, calculated on a total weight basis of 100 parts, include:

[0190] (1) Diisocyanate: diphenylmethane diisocyanate, 32 parts;

[0191] (2) a mixture of PDMS-OH and CTPB in a molar ratio of 1.5:1, a total of 38 parts, wherein the structures of PDMS-OH and CTPB are the same as those of PDMS-OH and CTPB in Example 1, respectively;

[0192] (3) Other macromolecular diols: polytetrahydrofuran diol, number average molecular weight 2000 g / mol, 22 parts;

[0193] (4) Small molecule chain extender: 1,4-butanediol, 8 parts.

[0194] The preparation method comprises the following steps:

[0195] 1) uniformly mixing a mixture of PDMS-OH and CTPB, other macromolecular diols, and a small molecular chain extender to obtain a mixture;

[0196] 2) adding diisocyanate to the mixture of step 1), reacting at 100° C. for 2 minutes to obtain a thermoplastic polyurethane elastomer.

[0197] Test Case

[0198] The properties of the thermoplastic polyurethane elastomers prepared in the embodiments and comparative examples were tested; the results are shown in Table 1.

[0199] Table 1 Properties of thermoplastic polyurethane elastomer

[0200]

[0201]

[0202] Since PDMS-OH has an extremely low solubility parameter and extremely poor compatibility, the Si-TPU prepared with it has severe phase separation and the product is opaque, while CTPB has a large solubility parameter and is reacted with PDMS-OH to prepare a polybutadiene silicone diol with a moderate solubility parameter. The thermoplastic polyurethane elastomer prepared by combining PDMS-OH, CTPB and diisocyanate in Comparative Example 4 has severe phase separation and poor mechanical properties, which is not conducive to the later processing of the product, and has high haze and poor transparency, which affects the use of the product. The Si-TPU prepared by the polybutadiene silicone diol provided by Examples 1-9 of the present invention has a smaller degree of phase separation, good mechanical properties and good product transparency.

[0203] Moreover, compared with the comparative examples, the tensile strength, elongation at break and hardness of the thermoplastic polyurethane elastomers provided in Examples 1-9 of the present invention are significantly improved, indicating that the thermoplastic polyurethane elastomer also has excellent mechanical properties. Compared with the comparative examples, the glass transition temperature of the thermoplastic polyurethane elastomers provided in Examples 1-9 of the present invention is significantly reduced and the static water contact angle is significantly improved, indicating that the thermoplastic polyurethane elastomer also has outstanding low-temperature resilience and surface hydrophobicity, and the thermoplastic polyurethane elastomer prepared in Example 1 has the best comprehensive performance.

[0204] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A polybutadiene silicone diol, characterized in that: Its structural formula is shown in formula (I): Wherein, m is an integer of 1-23, x is an integer of 1-17, y is an integer of 1-8, n is an integer of 2-12, and R1 is one of an alkyl group, an ether group, and an ester group containing 1-8 carbon atoms.

2. The polybutadiene silicone diol according to claim 1, characterized in that: m is an integer of 2-15; and / or, x is an integer of 2-9; and / or, y is an integer of 2-6; and / or, n is an integer of 4-10.

3. The polybutadiene silicone diol according to claim 1, characterized in that: R1 is -CH2-, -CH2CH2-, -CH2CH2CH2-, #-CH2OCH2CH2-*, -CH2CH2OCH2CH2-, *-CH2CH2OCH2CH2CH2-#, #-CH2COOCH2CH2-* or #-CH2CH2CH2COOCH2CH2CH2CH2-*, wherein the * end is connected to the oxygen atom and the # end is connected to the silicon atom.

4. The polybutadiene organosilicon diol according to any one of claims 1 to 3, characterized in that The polybutadiene silicone diol has a hydroxyl value of 5.3-29.1 mgKOH / g and an acid value of 0.01-0.5 mgKOH / g.

5. A method for preparing polybutadiene organosilicon diol, characterized in that: The method comprises the following steps: mixing carboxyl-terminated polybutadiene and hydroxyl-terminated polydimethylsiloxane, and subjecting the mixture to polycondensation to obtain polybutadiene silicone diol; the carboxyl-terminated polybutadiene has a structural formula as shown in formula (II), and the hydroxyl-terminated polydimethylsiloxane has a structural formula as shown in formula (III). Wherein, m, x, y in formula (II) and formula (III) are the same as defined in claim 1 or 2, and R1 in formula (III) is the same as defined in claim 1 or 3.

6. The method for preparing polybutadiene organosilicon diol according to claim 5, characterized in that: The molar ratio of the terminal hydroxyl polydimethylsiloxane to the terminal carboxyl polybutadiene is 1 to 2.5:1; and / or, during the polycondensation reaction, the system is first heated to 140-230° C. under the protection of an inert gas for reaction for 2-6 hours, then continuously heated to 210-280° C. for reaction for 2-8 hours, and then the vacuum system is turned on for reaction under vacuum conditions.

7. A thermoplastic silicone polyurethane elastomer, characterized in that: The raw materials for preparation thereof include the polybutadiene silicone diol described in any one of claims 1 to 4 or the polybutadiene silicone diol prepared by the preparation method described in claim 5 or 6; preferably, based on 100 parts by weight of the total raw materials, the raw materials for preparation of the thermoplastic silicone polyurethane elastomer include the following components: (1) diisocyanate: 19 to 42 parts, preferably 28 to 38 parts; (2) the polybutadiene silicone diol: 28 to 57 parts, preferably 34 to 47 parts; (3) other diols: 6 to 44 parts, preferably 15 to 27 parts; (4) Chain extender: 4 to 15 parts, preferably 5 to 9 parts.

8. The thermoplastic silicone polyurethane elastomer according to claim 7, characterized in that: The thermoplastic silicone polyurethane elastomer further satisfies at least one of the following (1)-(4): (1) The diisocyanate is one or more of aliphatic, alicyclic and aromatic diisocyanates; preferably at least one of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, p-phenylene diisocyanate, naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, xylylene diisocyanate, cyclohexane dimethylene diisocyanate, trimethyl-1,6-hexamethylene diisocyanate, tetramethyl meta-xylylene diisocyanate, norbornane diisocyanate, dimethyl biphenyl diisocyanate, methylcyclohexyl diisocyanate, dimethyl diphenylmethane diisocyanate and lysine diisocyanate; (2) the number average molecular weight of the other diol is 800-8000 g / mol, preferably 1000-6000 g / mol; (3) The other diols are other macromolecular diols having two terminal hydroxyl groups; preferably, the other diols are one or more of aliphatic or aromatic polyester diols, aliphatic or aromatic polyether diols, aliphatic or aromatic polycarbonate diols, aliphatic or aromatic polylactic acid diols, and aliphatic or aromatic polyolefin diols; more preferably, the other diols are one or more of polytetrahydrofuran diol, polybutylene adipate diol, polycarbonate diol, poly(1,6-hexanediol terephthalate) diol, polyoxypropylene diol, and polyethylene adipate diol; (4) The chain extender is a small molecule chain extender, preferably an aliphatic and / or aromatic small molecule chain extender; more preferably ethylene glycol, 1,4-butanediol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, neopentyl glycol, methyl propylene glycol, 1,6-hexanediol, 1,3-propylene glycol, dipropylene glycol, tripropylene glycol, butyl ethyl propylene glycol, diethyl pentanediol, 3-methyl-1,5-pentanediol, 1,3-butanediol, 1,2-butanediol, 2,3-butanediol, trimethyl pentanediol, 1,5-pentanediol, 1,2-pentanediol, hydroxy neopentyl glycol, 1,6-hexanediol, 1,3-propanediol ... One or more of hydroxyneopentyl valerate, 2-ethyl-1,3-hexanediol, dodecanediol, 1,4-dihydroxymethylcyclohexane, 1,4-cyclohexanediol, hydroquinone dihydroxyethyl ether, resorcinol dihydroxyethyl ether, resorcinol bishydroxypropyl ether, resorcinol bishydroxypropyl ethyl ether, 4-hydroxyethyloxyethyl-1-hydroxyethylphenylene diether, 3-hydroxyethyloxyethyl-1-hydroxyethylphenylene diether, bisphenol A dihydroxyethyl ether, bisphenol A dihydroxypropyl ether, 1,4-cyclohexanediamine, diaminodicyclohexylmethane, trimethylhexanediamine, and dimethyldiaminodicyclohexylmethane.

9. A method for preparing the thermoplastic silicone polyurethane elastomer according to claim 7 or 8, comprising the following steps: The polybutadiene silicone diol, other diols and a chain extender are mixed to obtain a mixture; the mixture is mixed with diisocyanate to react to obtain a thermoplastic silicone polyurethane elastomer; Optionally, the reaction temperature is 80-160°C.

10. Use of the thermoplastic silicone polyurethane elastomer according to claim 7 or 8 or the thermoplastic silicone polyurethane elastomer prepared by the preparation method according to claim 9 in medical supplies, clothing products, protective products, smart wearable devices, cables, and automotive products.

Citation Information

Patent Citations

  • Preparation method of two-component normal-temperature non-cured asphalt polyurethane waterproof coating

    CN112920701A

  • Polybutyronitrile organosilicon dihydric alcohol and preparation method thereof, and transparent thermoplastic organosilicon polyurethane elastomer and application thereof

    CN114634624A

  • Polysiloxane dihydric alcohol, thermoplastic organic silicon polyurethane elastomer, cross-linked polyurethane elastomer and application of polysiloxane dihydric alcohol, thermoplastic organic silicon polyurethane elastomer and cross-linked polyurethane elastomer

    CN114805813A