Organometal structure having excellent VOC adsorption and differential
Through the zirconium-based organometallic structure composed of fumaric acid and L-aspartic acid, the problems of insufficient VOC adsorption performance and poor anti-degassing performance in the prior art are solved, and the effects of efficient adsorption and low degassing rate are achieved. .
Patent Information
- Application Number
- CN202410525948.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-18
- Filing Date
- 2024-04-29
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art does not perform well in removing volatile organic compounds (VOCs), especially the adsorption performance of formaldehyde and anti-degassing properties. Activated carbon has insufficient VOC removal performance and there is a problem of adsorbent reversion. Although MIL-125MOF is improved Adsorption performance but poor degassing performance.
A zirconium-based organometallic structure using fumaric acid and L-aspartic acid as organic linkers is formed by adjusting its mixing ratio and synthesis process to form an organometallic structure with excellent adsorption performance and improved anti-degassing performance.
It achieves high efficiency adsorption and low degassing rate of VOC, significantly improving the adsorption performance of formaldehyde and anti-degassing performance, which is better than traditional activated carbon and MIL-125MOF.
Smart Images

Figure BDA0004816642830000131 
Figure BDA0004816642830000141 
Figure BDA0004816642830000151
Abstract
Description
Technical Field
[0001] The present invention relates to an organic metal structure having excellent adsorption performance for volatile organic compounds (VOCs) and excellent anti-degassing performance for the adsorbed VOCs, and a product comprising the organic metal structure. Background Art
[0002] There is a need to improve the formaldehyde adsorption performance and the anti-outgassing performance for the adsorbed formaldehyde.
[0003] However, in the case of activated carbon that has been used for removing VOCs as well as for removing particles (dust), for example, a 25-pyeong air purifier can process 25 pyeong of particles (dust), but can only process about 5 pyeong of VOCs, and therefore, the removal performance for VOCs is significantly insufficient compared to its removal performance for particles (dust). In addition, activated carbon causes degassing of adsorbed VOCs, so when the filter is used for a long time, there is a problem of recovery of adsorbed VOCs.
[0004] Meanwhile, the following patent document discloses a technology for improving the low VOC adsorption performance of activated carbon by adsorbing formaldehyde using MIL-125MOF (titanium-based organometallic structure). However, MIL-125MOF has a VOC adsorption performance superior to that of activated carbon, but has a degassing performance inferior to that of activated carbon, so the problem of adsorbed VOC recovery when using a filter has not been solved.
[0005] [Prior art literature]
[0006] [Patent Document]
[0007] (Patent Document 1) Korean Patent Laid-Open Publication No. 2023-0033579 Summary of the invention
[0008] The present invention provides an organic metal structure having excellent adsorption performance for VOC and improved anti-degassing performance for the adsorbed VOC.
[0009] As means for solving the above-mentioned problems, the present invention provides the following organometallic structures (1) to (6) and products (7) and (8).
[0010] (1) An organometallic structure, which is a zirconium-based organometallic structure (MOF) containing fumaric acid as an organic linker, and has excellent adsorption performance and anti-degassing performance for volatile organic compounds.
[0011] (2) In the above (1), the organometallic structure further includes L-aspartic acid as an organic linker.
[0012] (3) In the above (2), the mixing ratio of fumaric acid to L-aspartic acid is 9.5:0.5 to 0.1:9.9, 9:1 to 1:9, 8.5:1.5 to 1.5:8.5, 8:2 to 2:8, 7.5:2.5 to 2.5:7.5 or 7:3 to 3:7.
[0013] (4) In any one of the above (1) to (3), the organic metal structure has a crystal structure, and the size of the pore entrance formed by the crystal structure is larger than the size of the pore interior.
[0014] (5) In the above (4), the amine group (NH 2 ) is located in the hole.
[0015] (6) In any one of (1) to (5), the organic metal structure has a VOC adsorption rate of 95% or more and a degassing rate of 2.5% or less.
[0016] (7) A product comprising the organometallic structure according to any one of (1) to (6).
[0017] (8) In the above (7), the product includes a filter.
[0018] Beneficial effects
[0019] Compared with general organic metal structures, the organic metal structure of the present invention has improved VOC adsorption performance and improved anti-degassing performance of adsorbed VOC. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 shows images of organometallic structures synthesized according to Examples 1 to 10 of the present invention and Comparative Example 2;
[0021] Figure 2 PXRD analysis results of the organometallic structures synthesized according to Examples 1 to 10 and Comparative Example 2 of the present invention are shown;
[0022] Figure 3 The evaluation results of formaldehyde adsorption and anti-degassing performance of the organometallic structures according to Example 6 and Comparative Example 1 (MIL-125) are shown;
[0023] Figure 4 The evaluation results of formaldehyde adsorption and anti-degassing performance of the organometallic structures of Examples 1 to 10 and Comparative Example 2 are shown;
[0024] Figure 5 shows images of organometallic structures synthesized according to Examples 11 to 14 of the present invention;
[0025] Figure 6shows the PXRD analysis results of the organometallic structures synthesized according to Examples 11 to 14 of the present invention;
[0026] Figure 7 The evaluation results of formaldehyde adsorption and anti-degassing performance of the organometallic structures of Examples 11 to 14 are shown. DETAILED DESCRIPTION
[0027] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0028] However, the embodiments of the present invention shown below may be modified into other various forms, and the scope of the present invention is not limited to the embodiments described below. The embodiments of the present invention are provided to more fully describe the present invention to those skilled in the art.
[0029] [Example 1]
[0030] The organometallic structure of Example 1 was synthesized by the following process using the raw materials shown in Table 1 below.
[0031] [Table 1]
[0032] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid - - Fumaric Acid 24.37 75.6 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0033] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0034] Thereafter, 12.19 g (0.21 mol) of fumaric acid was added thereto and stirred. The final solution was subjected to reflux reaction at 120° C. for 24 hours to synthesize the organic metal structure of Example 1 (InCube 206 (0:10)). After the synthesis was completed, Buchner filtration was performed and washed with water and ethanol. After washing, vacuum drying was performed in an oven at 110° C. to obtain a white powdery organic metal structure.
[0035] Since the formic acid used in Table 1 is a substance used as a solvent, it is not substantially included in the obtained organic metal structure, but a small amount of formic acid may remain as an impurity during the synthesis process. This is the same for the organic metal structures obtained according to the following Examples 2 to 14.
[0036] [Example 2]
[0037] The organometallic structure of Example 2 was synthesized by the following process using the raw materials shown in Table 2 below.
[0038] [Table 2]
[0039] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 2.80 8.68 parts by weight Fumaric Acid 21.94 68.1 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0040] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0041] Thereafter, 2.80 g (0.021 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 21.94 g (0.189 mol) of fumaric acid was added thereto and then stirred. The final solution was refluxed at 120 ° C for 24 hours to synthesize the organic metal structure (InCube 206 (1: 9)) of Example 2. After the synthesis is completed, Buchner filtration is performed and washed with water and ethanol. After washing, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0042] [Example 3]
[0043] The organometallic structure of Example 3 was synthesized by the following process using the raw materials shown in Table 3 below.
[0044] [Table 3]
[0045] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 5.59 17.3 parts by weight Fumaric Acid 19.5 60.5 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0046] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0047] Thereafter, 5.59 g (0.042 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 19.5 g (0.168 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to reflux reaction at 120 ° C for 24 hours to synthesize the organic metal structure (InCube 206 (2: 8)) of Example 3. After the synthesis is completed, Buchner filtration is performed and washed with water and ethanol. After washing is completed, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0048] [Example 4]
[0049] The organometallic structure of Example 4 was synthesized by the following process using the raw materials shown in Table 4 below.
[0050] [Table 4]
[0051] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 8.39 26.0 parts by weight Fumaric Acid 17.06 52.9 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0052] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0053] Thereafter, 8.39 g (0.063 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 17.06 g (0.147 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to reflux reaction at 120 ° C for 24 hours to synthesize the organic metal structure (InCube 206 (3: 7)) of Example 4. After the synthesis was completed, Buchner filtration was performed and washed with water and ethanol. After washing, vacuum drying was performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0054] [Example 5]
[0055] The organometallic structure of Example 5 was synthesized by the following process using the raw materials shown in Table 5 below.
[0056] [Table 5]
[0057] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 11.18 34.7 parts by weight Fumaric Acid 14.63 45.4 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0058] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0059] Thereafter, 11.18 g (0.084 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 14.63 g (0.126 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to reflux reaction at 120 ° C for 24 hours to synthesize the organic metal structure (InCube 206 (4: 6)) of Example 5. After the synthesis is completed, Buchner filtration is performed and washed with water and ethanol. After washing is completed, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0060] [Example 6]
[0061] The organometallic structure of Example 6 was synthesized by the following process using the raw materials shown in Table 6 below.
[0062] [Table 6]
[0063] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 13.98 43.4 parts by weight Fumaric Acid 12.19 37.8 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0064] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0065] Thereafter, 13.98 g (0.105 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 12.19 g (0.105 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to a 24-hour reflux reaction at 120 ° C to synthesize the organic metal structure of Example 6 (InCube 206 (5:5)). After the synthesis is completed, Buchner filtration is performed and washed with water and ethanol. After washing is completed, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0066] [Example 7]
[0067] The organometallic structure of Example 7 was synthesized by the following process using the raw materials shown in Table 7 below.
[0068] [Table 7]
[0069] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 16.77 52.0 parts by weight Fumaric Acid 9.75 30.3 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0070] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0071] Thereafter, 16.77 g (0.126 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 9.75 g (0.084 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to reflux reaction at 120 ° C for 24 hours to synthesize the organic metal structure (InCube 206 (6: 4)) of Example 7. After the synthesis is completed, Buchner filtration is performed and washed with water and ethanol. After washing is completed, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0072] [Example 8]
[0073] The organometallic structure of Example 8 was synthesized by the following process using the raw materials shown in Table 8 below.
[0074] [Table 8]
[0075] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 19.57 60.7 parts by weight Fumaric Acid 7.31 22.7 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0076] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0077] Thereafter, 19.57 g (0.147 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 7.31 g (0.063 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to a 24-hour reflux reaction at 120 ° C to synthesize the organic metal structure of Example 8 (InCube 206 (7: 3)). After the synthesis was completed, Buchner filtration was performed and washed with water and ethanol. After washing, vacuum drying was performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0078] [Example 9]
[0079] The organometallic structure of Example 9 was synthesized by the following process using the raw materials shown in Table 9 below.
[0080] [Table 9]
[0081] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 22.36 69.4 parts by weight Fumaric Acid 4.87 15.1 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0082] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0083] Thereafter, 22.36 g (0.168 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 4.87 g (0.042 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to reflux reaction at 120 ° C for 24 hours to synthesize the organic metal structure of Example 9 (InCube 206 (8: 2)). After the synthesis is completed, Buchner filtration is performed and washed with water and ethanol. After washing is completed, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0084] [Example 10]
[0085] The organometallic structure of Example 10 was synthesized by the following process using the raw materials shown in Table 10 below.
[0086] [Table 10]
[0087] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 25.16 78.1 parts by weight Fumaric Acid 2.44 7.57 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0088] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0089] Thereafter, 25.16 g (0.189 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 2.44 g (0.021 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to reflux reaction at 120 ° C for 24 hours to synthesize the organic metal structure (InCube 206 (9: 1)) of Example 10. After the synthesis is completed, Buchner filtration is performed and washed with water and ethanol. After washing, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0090] [Example 11]
[0091] The organometallic structure of Example 11 was synthesized by the following process using the raw materials shown in Table 11 below.
[0092] [Table 11]
[0093] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 26.55 82.38 parts by weight Fumaric Acid 1.22 3.79 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0094] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0095] Thereafter, 26.55 g (0.1995 mol) of L-aspartic acid was added thereto and then completely dissolved. Finally, 1.22 g (0.0105 mol) of fumaric acid was added thereto and then stirred. The final solution was subjected to reflux reaction at 120 ° C for 24 hours to synthesize the organic metal structure of Example 11 (InCube 206 (0.5:9.5)). After the synthesis is completed, Buchner filtration is performed and washed with water and ethanol. After washing is completed, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0096] [Example 12]
[0097] The organometallic structure of Example 12 was synthesized by the following process using the raw materials shown in Table 12 below.
[0098] [Table 12]
[0099] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 26.83 83.25 parts by weight Fumaric Acid 0.97 3.01 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0100] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0101] Thereafter, 26.83 g (0.2016 mol) of L-aspartic acid was added thereto, and then completely dissolved. Finally, 0.97 g (0.0084 mol) of fumaric acid was added thereto, and then stirred. The final solution was subjected to reflux reaction at 120° C. for 24 hours to synthesize the organic metal structure of Example 12 (InCube 206 (0.4:9.6)). After the synthesis was completed, Buchner filtration was performed, and water and ethanol were used for washing. After washing, vacuum drying was performed in an oven at 110° C. to obtain a white powdery organic metal structure.
[0102] [Example 13]
[0103] The organometallic structure of Example 13 was synthesized by the following process using the raw materials shown in Table 13 below.
[0104] [Table 13]
[0105] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 27.11 84.11 parts by weight Fumaric Acid 0.73 2.26 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0106] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0107] Thereafter, 27.11 g (0.2037 mol) of L-aspartic acid was added thereto, and then completely dissolved. Finally, 0.73 g (0.0063 mol) of fumaric acid was added thereto, and then stirred. The final solution was subjected to reflux reaction at 120° C. for 24 hours to synthesize the organic metal structure of Example 13 (InCube 206 (0.3:9.7)). After the synthesis was completed, Buchner filtration was performed, and water and ethanol were used for washing. After washing, vacuum drying was performed in an oven at 110° C. to obtain a white powdery organic metal structure.
[0108] [Example 14]
[0109] The organometallic structure of Example 14 was synthesized by the following process using the raw materials shown in Table 14 below.
[0110] [Table 14]
[0111] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 27.67 85.85 parts by weight Fumaric Acid 0.24 0.75 parts by weight Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0112] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0113] Thereafter, 27.67 g (0.2079 mol) of L-aspartic acid was added thereto, and then completely dissolved. Finally, 0.24 g (0.0021 mol) of fumaric acid was added thereto, and then stirred. The final solution was subjected to reflux reaction at 120 ° C for 24 hours to synthesize the organic metal structure of Example 14 (InCube 206 (0.1:9.9)). After the synthesis is completed, Buchner filtration is performed, and water and ethanol are used for washing. After washing is completed, vacuum drying is performed in an oven at 110 ° C to obtain a white powdery organic metal structure.
[0114] [Example 15]
[0115] In order to measure the formaldehyde absorption / degassing performance of the organometallic structures of Examples 1 to 14, suspensions were prepared using the organometallic structures of Examples 1 to 14, respectively, and the suspensions were subjected to roll-to-roll coating as known in the art, and then dried. At this time, the amount of sample loaded on the coated sheet was 100 μm / 1 m 2 Sheet 30-100g.
[0116] [Comparative Example 1]
[0117] For comparison with Examples 1 to 10, MIL125 MOF was synthesized by the following process.
[0118] 0.5g (0.003mol) of terephthalic acid was added to DMF / MeOH (9 / 1mL) and then completely dissolved. 0.26ml (0.0008mol) of titanium butoxide was added to the solution prepared above and then stirred. The mixture was transferred to a 20ml Teflon container, placed in an autoclave, and then heated to 150°C for 24 hours. After the synthesis was completed, a centrifuge was used for primary filtration, and DMF and MeOH were each washed three times. After washing was completed, vacuum drying was performed in an oven at 80°C to obtain a white powdery organic metal structure.
[0119] [Comparative Example 2]
[0120] The organometallic structure of Comparative Example 2 was synthesized by the following procedure using the raw materials shown in Table 15 below.
[0121] [Table 15]
[0122] Material Name Weight(g) Remark <![CDATA[Zirconium oxychloride (ZrOCl 2 ·8H 2 O)]]> 32.23 100 parts by weight L-Aspartic Acid 27.95 86.7 parts by weight Fumaric Acid - - Formic acid 92.06 285.6 parts by weight Distilled water (DI) 100 310.3 parts by weight
[0123] 32.23 g (0.1 mol) of zirconium (IV) oxychloride was added to 100 ml of distilled water, and then completely melted. 92.06 g of formic acid was added to the above-prepared solution, and then stirred.
[0124] Thereafter, 27.95 g (0.21 mol) of L-aspartic acid was added thereto and then completely dissolved. The final solution was subjected to reflux reaction at 120° C. for 24 hours to synthesize the organic metal structure of Comparative Example 2 (InCube 206 (0:10)). After the synthesis was completed, Buchner filtration was performed and washed with water and ethanol. After washing, vacuum drying was performed in an oven at 110° C. to obtain a white powdery organic metal structure.
[0125] [Comparative Example 3]
[0126] As a method for preparing a sample for measuring the formaldehyde absorption / degassing performance of the organometallic structures of Comparative Examples 1 and 2, a suspension was prepared using the organometallic structure of Comparative Example 1, and the suspension was subjected to roll-to-roll coating as known in the art, and then dried. At this time, the amount of the sample loaded on the coating sheet was 100 μm / 1 m 2 Sheet 30-50g.
[0127] Figure 1 1 and 2 show images of the organometallic structures synthesized according to Examples 1 to 10 of the present invention and Comparative Example 2. Figure 1 As shown, the organometallic structures synthesized according to Examples 1 to 10 and Comparative Example 2 are formed in a particle phase having a size of about several nanometers to several hundred nanometers.
[0128] Figure 2 The PXRD analysis results of the organometallic structures synthesized according to Examples 1 to 10 and Comparative Example 2 of the present invention are shown. Figure 2 As shown, it was confirmed by PXRD analysis that the organometallic structures synthesized according to Examples 1 to 10 and Comparative Example 2 were formed in a crystalline phase.
[0129] Figure 3 The results of analysis of formaldehyde adsorption and anti-degassing performance of samples prepared by roll-to-roll coating of the organometallic structure powders synthesized in Example 6 of the present invention and Comparative Example 1 (MIL-125, indicated as "existing material" in the figure) are shown. Figure 3 As shown, it can be confirmed that the formaldehyde adsorption and degassing performance of the sample of Example 6 is superior to the formaldehyde adsorption and degassing performance of the existing samples.
[0130] The formaldehyde adsorption and degassing performance was evaluated in ppm using a cyclic adsorption measurement system. At this time, a formaldehyde gas of a specific concentration was prepared and passed through a roll-to-roll coated sample in a chamber of the measurement system, and then the concentration change in the chamber was tracked, thereby obtaining a formaldehyde adsorption isotherm. In order to measure the adsorption performance, formaldehyde gas of about 20 ppm or less was passed through the sample and the formaldehyde adsorption amount was measured for 20 minutes. In addition, after adsorption, the amount of formaldehyde generated from the sample was measured for 20 minutes by introducing a gas without formaldehyde, thereby measuring the amount of re-degassing from the sample.
[0131] Figure 4 The evaluation results of formaldehyde adsorption and anti-degassing performance of the organometallic structures of Examples 1 to 10 and Comparative Example 2 are shown.
[0132] like Figure 4 As shown in , Examples 2 to 10 have formaldehyde adsorption and anti-degassing properties superior to those of the existing material as Comparative Example 1, and it can be seen that Examples 4 to 8 in particular have adsorption and anti-degassing properties significantly improved compared to the existing material.
[0133] Figure 5 1 and 2 show images of the organometallic structures synthesized according to Examples 11 to 14 of the present invention. Figure 5 As shown, the organometallic structures synthesized according to Examples 11 to 14 are formed in a particle phase having a size of about several nanometers to several hundred nanometers.
[0134] Figure 6 1 and 2 show the PXRD analysis results of the organometallic structures synthesized according to Examples 11 to 14 of the present invention. Figure 6 As shown, it was confirmed by PXRD analysis that the organometallic structures synthesized according to Examples 11 to 14 were formed in a crystalline phase.
[0135] Figure 7 The evaluation results of the formaldehyde adsorption and anti-degassing performance of the organometallic structures of Examples 11 to 14 are shown. Figure 7 As shown, compared with Comparative Example 1, Examples 11 to 14 have excellent formaldehyde adsorption and anti-degassing performance.
[0136] Table 16 is Figure 4 and 7 The results are numerically expressed, and the results summarizing the formaldehyde adsorption amount and adsorption rate and the formaldehyde degassing amount and degassing rate are shown.
[0137] [Table 16]
[0138]
[0139]
[0140]
[0141] As shown in Table 16, compared with MIL-125 previously developed to improve the adsorption performance of VOCs, Examples 1 to 14 of the present invention have higher formaldehyde adsorption amounts and lower formaldehyde degassing rates.
[0142] Meanwhile, in the case of Comparative Example 2 containing no fumaric acid, the adsorption amount of formaldehyde was increased compared to MIL-125MPa, and the degassing rate of formaldehyde was further increased.
[0143] In the embodiments of the present invention, it can be seen that Embodiment 4 (InCube 206 (7:3)) to Embodiment 8 (InCube 206 (3:7)) particularly have high formaldehyde adsorption rates and low formaldehyde degassing rates, and thus have more ideal performance.
Claims
1. An organic metal structure, which is a zirconium-based organic metal structure (MOF) containing fumaric acid as an organic linker, and has excellent adsorption performance and anti-degassing performance for volatile organic compounds. 2 . The organometallic structure according to claim 1 , further comprising L-aspartic acid as an organic linker.
3. The organic metal structure according to claim 2, wherein the mixing molar ratio of fumaric acid to L-aspartic acid is 9.5:0.5 to 0.1:9.
9.
4. The organic metal structure according to claim 2, wherein the mixing molar ratio of fumaric acid to L-aspartic acid is 9:1 to 1:
9.
5. The organic metal structure according to claim 2, wherein the mixing molar ratio of fumaric acid to L-aspartic acid is 7.5:2.5 to 2.5:7.
5. 6 . The organic metal structure according to claim 1 , wherein the organic metal structure has a crystal structure, and a size of a pore entrance formed by the crystal structure is larger than a size of an interior of the pore.
7. The organometallic structure of claim 6, wherein the amine groups (NH2) are located within the pores. 8 . The organic metal structure according to claim 1 , wherein the organic metal structure has a VOC adsorption rate of 95% or more and a degassing rate of 2.5% or less. 9 . An article comprising the organometallic structure according to claim 1 .