Full-biodegradable mulching film special for rice, preparation method and application

Through the use of modified nano calcium carbonate, the problems of poor dispersion of nano calcium carbonate and increased soil pH in rice-specific mulching films were solved, and soil pH balance and improved biodegradability of mulching films were achieved, which promoted crop growth and environmental protection.

CN118930914APending Publication Date: 2024-11-12JIANGSU DAOYUE AGRICULTURAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411037443.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Nano calcium carbonate has poor dispersion in the plastic film for whole biodegradable rice and can easily lead to an increase in soil pH, affecting crop growth.

Method used

Modified nano calcium carbonate is used to improve its dispersion in the PBAT-PLA system through amino acid modification, and neutralize OH-ions during natural decomposition to balance the soil pH.

Benefits of technology

It significantly improves the dispersion performance of nano calcium carbonate, stabilizes the soil pH value, promotes healthy circulation of the soil microenvironment, enhances the biodegradability and mechanical properties of the mulch film, and improves crop yield and quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a full-biodegradable mulching film special for rice, a preparation method and application. The preparation method comprises the following steps: S1, weighing the following raw materials in percentage by weight: 50-65% of PBAT, 10-20% of modified nano calcium carbonate, 5-20% of PLA, 5-15% of polytrimethylene terephthalate (PTT), 0.2-2% of a hydrolysis-resistant agent, 0.2-2% of an antioxidant, 0.2-2% of a light stabilizer, 0.5-5% of a lubricant and 1-5% of an anti-blocking agent; s2, putting the weighed raw materials into a double-screw extruder for extrusion modification and granulation to obtain mixed particles; and S3, carrying out blow molding on the mixed particles by a film blowing machine to obtain the full-biodegradable mulching film special for rice. The modified nano calcium carbonate is adopted to replace traditional calcium carbonate, the dispersing performance is improved, and when the modified nano calcium carbonate is naturally decomposed, amino acid on the surface of the modified nano calcium carbonate can release H < + > to neutralize OH <->, so that the pH value of soil is balanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of weed control film, in particular to a fully biodegradable rice-specific film, a preparation method and application thereof. Background Art

[0002] In the context of sustainable development of modern agriculture, fully biodegradable rice mulch, as an innovative agricultural technology, is gradually becoming a preferred alternative to traditional plastic mulch. Although traditional plastic mulch has effectively improved crop yield and quality, its difficult-to-degrade nature has led to serious "white pollution" in farmland. To meet this challenge, researchers have developed fully biodegradable mulch, which is mainly composed of environmentally friendly materials such as biodegradable polymers such as polybutylene succinate (PBAT) and polylactic acid (PLA). It aims to provide similar functions as traditional plastic mulch, such as heat preservation and moisture retention, and inhibition of weed growth. At the same time, after the crop growth cycle ends, it can be quickly degraded into harmless substances such as water and carbon dioxide under natural conditions, effectively reducing environmental pollution.

[0003] In the formulation design of fully biodegradable rice mulch, nano calcium carbonate is widely used as a common filler to reduce costs and improve the physical properties of the mulch. Nano calcium carbonate can not only improve the mechanical strength and weather resistance of the mulch, but also enhance the light transmittance of the mulch through its good light scattering effect, which is beneficial to rice growth. In addition, as a natural mineral source, it is more environmentally friendly than synthetic fillers and conforms to the green concept of biodegradable materials.

[0004] However, the application of nano-calcium carbonate is not without controversy. On the one hand, in the preparation process of fully biodegradable rice mulch, due to its high surface energy and strong hydrophilicity, nano-calcium carbonate is difficult to disperse in the PBAT-PLA system and easily forms agglomerates. On the other hand, a large amount of nano-calcium carbonate remains in the soil and produces hydroxide ions through hydrolysis, which will lead to an unnatural increase in soil pH, that is, an increase in alkalinity. The imbalance of soil pH directly affects the effectiveness of nutrients in the soil, which in turn affects the normal growth and development of crops. Summary of the invention

[0005] In view of the problem that nano calcium carbonate has poor dispersibility and easily leads to increased soil alkalinity, the present invention provides a fully biodegradable rice-specific mulch film, a preparation method and an application thereof. Modified nano calcium carbonate is used to replace traditional calcium carbonate, which not only improves the dispersibility, but also the amino acids on the surface of the modified nano calcium carbonate can release H during natural decomposition. + To neutralize the OH produced by the hydrolysis of nano calcium carbonate - , thereby balancing the pH value of the soil.

[0006] The present invention achieves the above technical objectives through the following technical means.

[0007] A method for preparing a fully biodegradable rice mulch film, characterized in that it comprises the following steps:

[0008] S1: Weigh 50-65% of PBAT, 10-20% of modified nano calcium carbonate, 5-20% of PLA, 5-15% of polytrimethylene terephthalate (PTT), 0.2-2% of anti-hydrolysis agent, 0.2-2% of antioxidant, 0.2-2% of light stabilizer, 0.5-5% of lubricant and 1-5% of anti-blocking agent as raw materials by weight percentage;

[0009] The preparation method of the modified nano calcium carbonate is as follows: weigh a certain amount of nano calcium carbonate and disperse it in anhydrous ethanol to obtain a suspension; dissolve the amino acid in water, heat it for 0.5 to 1 hour, add the suspension drop by drop, and after cross-linking reaction for 2 to 3 hours, filter, wash and dry to obtain the modified nano calcium carbonate;

[0010] The anti-hydrolysis agent comprises monomeric carbodiimide and phenyl glycidyl ether, and the ratio of the two is 1:(1-5);

[0011] S2: placing the weighed raw materials in a twin-screw extruder for extrusion modification and granulation to obtain mixed granules;

[0012] S3: The mixed particles are blown by a film blowing machine to obtain a fully biodegradable rice-specific mulch film.

[0013] Furthermore, in step S1, the weight percentages of the PBAT, modified nano-calcium carbonate and PLA are 60-65%, 15-20% and 5-15% respectively; the ratio of monomeric carbodiimide and phenyl glycidyl ether in the hydrolysis resistance agent is 1:(1-3).

[0014] Furthermore, the heating temperature of the amino acid is 250-350°C;

[0015] Furthermore, the amino acid is one or more of lysine, arginine, histidine, alanine, glycine, valine, leucine, isoleucine, proline, phenylalanine, tryptophan, methionine, serine, threonine, cysteine, tyrosine, asparagine, glutamine, and the like.

[0016] Furthermore, the antioxidant is one or a combination of antioxidant 1010 or antioxidant 168; the light stabilizer is polyoxyethylene (20) sorbitan monostearate and light stabilizer UV-783, light stabilizer 622 or light stabilizer 119, and the ratio of polyoxyethylene (20) sorbitan monostearate to light stabilizer UV-783, light stabilizer 622 or light stabilizer 119 is 1:(20-30); the lubricant is stearic acid amide or erucic acid amide, and the opening agent is silicon dioxide powder or erucic acid amide.

[0017] Furthermore, in step S2, before placing the raw materials in the twin-screw extruder, the raw materials are first placed in a mixer for mixing for 2 to 4 minutes.

[0018] Furthermore, in step S2, the granulation temperature is 150-200°C, preferably 180-200°C; in step S3, the blow molding temperature is 150-200°C, preferably 180-200°C.

[0019] Furthermore, the molding thickness of the fully biodegradable rice-specific mulch film is 0.05 to 0.01 mm.

[0020] A fully biodegradable rice-specific mulch film prepared by any of the above preparation methods.

[0021] The above-mentioned fully biodegradable rice-specific mulch film is used in the field of crop planting.

[0022] In the present invention, the modification mechanism of the nano calcium carbonate is as follows: the amino acid molecules in the liquid phase are freed to the surface of the nano calcium carbonate particles to generate a poorly soluble salt precursor. 2+ The reaction generates insoluble salts, and at the same time, the insoluble salt precursors in the liquid phase migrate to the surface of the calcium carbonate particles. Finally, the insoluble salts in the main body of the liquid phase adsorb and grow on the surface of the calcium carbonate particles, coating the calcium carbonate particles, thereby achieving the purpose of surface modification.

[0023] The beneficial effects of the present invention are as follows:

[0024] 1. The present invention grafts amino acids onto the surface of modified nano-calcium carbonate by chemical bonding. On the one hand, the polarity and overall surface energy of the particle surface are reduced, which promotes the particles to achieve a higher level of stability in a dispersed state, significantly reduces the tendency of agglomeration between particles, and optimizes the dispersion characteristics of the material. On the other hand, amino acids can not only release hydrogen ions (H+) in the natural decomposition process to effectively neutralize the hydroxide ions (OH-) generated by the decomposition of calcium carbonate, but also chelate Ca in the soil. 2+, promoting the dissolution of calcium carbonate, thereby achieving the acid-base balance of the soil medium, which has a positive effect on maintaining the pH stability of the soil microenvironment and promoting the healthy circulation of the ecosystem.

[0025] 2. The amino acids attached to the surface of the modified nano-calcium carbonate in the present invention are natural organic molecules that are easily recognized and degraded by soil microorganisms, ensuring the overall biodegradability of the mulch film and being beneficial to ecological environmental protection. Amino acids can slowly release nutrients during the decomposition process, providing necessary trace elements for plant roots, and helping to improve the yield and quality of crops.

[0026] 3. The amino acids attached to the surface of the modified nano-calcium carbonate in the present invention can reduce the content of calcium carbonate in the soil, reduce the fixation of phosphorus by the soil, and improve the effectiveness of phosphate fertilizer.

[0027] 4. The present invention introduces calcium carbonate as an inorganic filling material for the mulch film, which not only significantly reduces the economic cost of mulch film production, but also due to the extremely high thermal stability of calcium carbonate, its addition can effectively improve the thermal stability of the mulch film. Calcium carbonate can also improve the rigidity, dimensional stability and hardness of the mulch film, enhance its mechanical properties, and make the mulch film more durable and more resistant to external damage.

[0028] 5. The monomeric carbodiimide in the present invention has the advantages of high activity and rapid onset, while phenyl glycidyl ether can react with the terminal carboxyl and terminal hydroxyl groups on the molecular chain of the ground film to form new chemical bonds, thereby not only playing a capping role, but also achieving chain extension and cross-linking of the molecular chain, and having the dual effects of improving the hydrolysis resistance and mechanical properties of the ground film. The synergistic use of the two materials ensures that the hydrolysis-resistant additive of the present invention can take effect quickly, while giving the ground film long-term stability and excellent mechanical properties, achieving the simultaneous improvement of protection efficiency and comprehensive material performance.

[0029] 6. The molecular structure of polytrimethylene terephthalate (PTT) in the present invention is compact, the crystallinity is high, and due to the characteristics of its hydrophobic functional groups, it has natural resistance to the absorption and penetration of water molecules, which can effectively prevent water molecules from entering the interior of the polymer, thereby significantly reducing the water absorption rate of the ground film. At the same time, due to the strong van der Waals force between PTT molecular chains and the high crystallinity, PTT can better transmit stress during stretching, and chain slip is not easy to occur, thereby improving the tensile strength of the material.

[0030] 7. The polyoxyethylene (20) sorbitan monostearate in the present invention can capture free radicals to a certain extent and reduce light-induced free radical chain reactions through its own antioxidant properties. It can also effectively reflect and scatter part of ultraviolet radiation, effectively improving the anti-ultraviolet ability of the ground film.

[0031] 8. The level of heavy metals contained in the fully biodegradable rice-specific mulch film of the present invention is far lower than the safety limit stipulated by the state, ensuring that the products after its decomposition in the soil do not pose any pollution risk to the surrounding environment and crops, thereby achieving dual protection of environmental protection and crop safety.

[0032] 9. The fully biodegradable rice mulch film of the present invention exhibits excellent heat preservation and moisture retention performance, creates a more ideal microclimate environment for rice, helps rice germinate earlier and grow vigorously, thereby achieving the goal of increasing production. This has great strategic significance for strengthening national food security. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0034] Example 1

[0035] The method for preparing the fully biodegradable rice mulch film described in this embodiment comprises the following steps:

[0036] S1: Weigh 60% PBAT, 15% modified nano calcium carbonate, 15% PLA, 5% polytrimethylene terephthalate (PTT), 2% hydrolysis resistance agent, 1% antioxidant, 0.5% light stabilizer, 0.5% lubricant and 1% anti-blocking agent by weight percentage.

[0037] The preparation method of the modified nano calcium carbonate is as follows: weigh a certain amount of nano calcium carbonate and disperse it in anhydrous ethanol to obtain a suspension; dissolve alanine in water, heat it for 1 hour, add the suspension dropwise, and after cross-linking reaction for 2 hours, filter, wash and dry to obtain the modified nano calcium carbonate.

[0038] S2: The weighed raw materials are placed in a mixer for 2 minutes of mixing, and then placed in a twin-screw extruder for extrusion modification and granulation at 180° C. to obtain mixed granules.

[0039] S3: The obtained mixed particles are blown by a film blowing machine at a blowing temperature of 180° C. to obtain a fully biodegradable rice-specific mulch film.

[0040] Furthermore, the anti-hydrolysis agent includes monomeric carbodiimide and phenyl glycidyl ether, and the ratio of the two is 1:3. The antioxidant is antioxidant 1010. The light stabilizer is polyoxyethylene (20) sorbitan monostearate and light stabilizer UV-783, and the ratio of the two is 1:20. The lubricant is stearic acid amide. The opening agent is silicon dioxide micropowder.

[0041] The performance of the above-prepared fully biodegradable rice-specific mulch film was tested, and the experimental methods and experimental results of each experimental item were as follows:

[0042] 1. Mechanical properties (tensile, nominal strain at break): According to GB / T 1040.3-2006 (Determination of tensile properties of plastics Part 3 Test conditions for films and sheets), the longitudinal / transverse tensile loads of the above-mentioned biodegradable mulch are measured to be 2.51N and 2.22N respectively. The test is qualified, which shows that the mulch has a certain mechanical strength and can withstand a certain external force without being easily damaged. The longitudinal / transverse nominal strains at break of the biodegradable mulch are 675% and 911% respectively, indicating that the mulch has extremely high ductility and toughness. It is not easy to break even when subjected to large deformation. It has strong adaptability and is conducive to dynamic changes during crop growth.

[0043] 2. Mechanical properties (right-angle tear): According to QB / T 1130-1991 (Test method for right-angle tear performance of plastics), the longitudinal / transverse right-angle tear loads of the above-mentioned biodegradable mulch film were measured to be 1.13N and 0.91N respectively. The test was qualified, which shows that the mulch film shows good resistance when subjected to tearing force, which is conducive to maintaining integrity when used in the field and reducing damage caused by external forces.

[0044] 3. Water vapor permeability: According to GB / T 1037-1988 (Test method for water vapor permeability of plastic film and sheet - cup method), the water vapor permeability of the above biodegradable mulch film is 392g / (m 2 ·24h), the test was qualified, which shows that the mulch film has strong water retention capacity and can promote the efficient use of water resources.

[0045] 4. Heavy metal content: According to GB / T 15337-2008 (General Rules for Atomic Absorption Spectrometry), the heavy metal content of the biodegradable mulch prepared above is: arsenic 0.502mg / kg, cadmium 0.403mg / kg, copper <0.01mg / kg, lead 3.57mg / kg, mercury <0.0002mg / kg, nickel 7.33mg / kg, selenium 0.274mg / kg, zinc <0.01mg / kg, chromium 0.644mg / kg, molybdenum 0.646mg / kg, fluorine 8.39mg / kg, cobalt <0.0006mg / kg. The heavy metal content is lower than or far lower than the national standard limit. The qualified test ensures that the degradation products of the mulch in the soil will not pollute the environment and crops.

[0046] 5. Organic content: According to GB / T 9345.1-2008 (Determination of ash content of plastics Part 1: General method), the biological organic content of the biodegradable mulch prepared above is 99%, and this test is qualified, which proves its environmental friendliness. According to GB / T19277.1-2011, the relative biodegradability rate (180d) of the biodegradable mulch is 97.6%.

[0047] Example 2

[0048] The method for preparing the fully biodegradable rice mulch film described in this embodiment comprises the following steps:

[0049] S1: Weigh 65% of PBAT, 20% of modified nano calcium carbonate, 5% of PLA, 5% of polytrimethylene terephthalate (PTT), 1% of hydrolysis resistance agent, 1% of antioxidant, 1% of light stabilizer, 1% of lubricant and 1% of anti-blocking agent by weight percentage.

[0050] The preparation method of the modified nano calcium carbonate is as follows: weigh a certain amount of nano calcium carbonate and disperse it in anhydrous ethanol to obtain a suspension; dissolve lysine in water, heat it for 1 hour, add the suspension drop by drop, and after cross-linking reaction for 3 hours, filter, wash and dry to obtain the modified nano calcium carbonate.

[0051] S2: The weighed raw materials are placed in a mixer for 2 minutes of mixing, and then placed in a twin-screw extruder for extrusion modification and granulation at 200° C. to obtain mixed granules.

[0052] S3: The obtained mixed particles are blown by a film blowing machine at a blowing temperature of 200° C. to obtain a fully biodegradable rice-specific mulch film.

[0053] Furthermore, the anti-hydrolysis agent includes monomeric carbodiimide and phenyl glycidyl ether, and the ratio of the two is 1:3. The antioxidant is antioxidant 1010. The light stabilizer is polyoxyethylene (20) sorbitan monostearate and light stabilizer UV-783, and the ratio of the two is 1:30. The lubricant is stearic acid amide, and the opening agent is silicon dioxide micropowder.

[0054] Example 3

[0055] The method for preparing the fully biodegradable rice mulch film described in this embodiment comprises the following steps:

[0056] S1: Weigh 55% of PBAT, 10% of modified nano calcium carbonate, 10% of PLA, 15% of polytrimethylene terephthalate (PTT), 2% of anti-hydrolysis agent, 2% of antioxidant, 2% of light stabilizer, 1% of lubricant and 3% of anti-blocking agent by weight percentage.

[0057] The preparation method of the modified nano calcium carbonate is as follows: weigh a certain amount of nano calcium carbonate and disperse it in anhydrous ethanol to obtain a suspension; dissolve leucine in water, heat it for 0.5 hours, and then dropwise add the suspension; after cross-linking reaction for 3 hours, filter, wash, and dry to obtain the modified nano calcium carbonate.

[0058] S2: The weighed raw materials are placed in a mixer for 2 minutes of mixing, and then placed in a twin-screw extruder for extrusion modification and granulation at 180° C. to obtain mixed granules.

[0059] S3: The obtained mixed particles are blown by a film blowing machine at a blowing temperature of 180° C. to obtain a fully biodegradable rice-specific mulch film.

[0060] Furthermore, the anti-hydrolysis agent includes monomeric carbodiimide and phenyl glycidyl ether, and the ratio of the two is 1:1. The antioxidant is antioxidant 1010. The light stabilizer is polyoxyethylene (20) sorbitan monostearate and light stabilizer 622, and the ratio of the two is 1:20. The lubricant is stearic acid amide, and the opening agent is silicon dioxide micropowder.

[0061] Example 4

[0062] The method for preparing the fully biodegradable rice mulch film described in this embodiment comprises the following steps:

[0063] S1: Weigh 50% PBAT, 20% modified nano calcium carbonate, 10% PLA, 10% polytrimethylene terephthalate (PTT), 2% hydrolysis resistance agent, 1% antioxidant, 1% light stabilizer, 2% lubricant and 4% anti-blocking agent by weight percentage.

[0064] The preparation method of the modified nano calcium carbonate is as follows: a certain amount of nano calcium carbonate is weighed and dispersed in anhydrous ethanol to obtain a suspension, phenylalanine is dissolved in water, heated for 1 hour, and then the suspension is added dropwise, and after a cross-linking reaction for 3 hours, the modified nano calcium carbonate is filtered, washed, and dried to obtain the modified nano calcium carbonate.

[0065] S2: The weighed raw materials are placed in a mixer for 2 minutes of mixing, and then placed in a twin-screw extruder for extrusion modification and granulation at 180° C. to obtain mixed granules.

[0066] S3: The obtained mixed particles are blown by a film blowing machine at a blowing temperature of 180° C. to obtain a fully biodegradable rice-specific mulch film.

[0067] Furthermore, the anti-hydrolysis agent includes monomeric carbodiimide and phenyl glycidyl ether, and the ratio of the two is 1:5. The antioxidant is antioxidant 1010. The light stabilizer is polyoxyethylene (20) sorbitan monostearate and light stabilizer 119, and the ratio of the two is 1:20. The lubricant is stearic acid amide, and the opening agent is silicon dioxide micropowder.

[0068] Example 5

[0069] The method for preparing the fully biodegradable rice mulch film described in this embodiment comprises the following steps:

[0070] S1: Weigh 65% PBAT, 10% modified nano calcium carbonate, 15% PLA, 5% polytrimethylene terephthalate (PTT), 0.5% hydrolysis resistance agent, 0.5% antioxidant, 1% light stabilizer, 1% lubricant, and 2% anti-blocking agent by weight percentage.

[0071] The preparation method of the modified nano calcium carbonate is as follows: a certain amount of nano calcium carbonate is weighed and dispersed in anhydrous ethanol to obtain a suspension, glycine is dissolved in water, the suspension is added dropwise after heating for 1 hour, and after cross-linking reaction for 2 hours, the modified nano calcium carbonate is filtered, washed and dried to obtain the modified nano calcium carbonate.

[0072] S2: The weighed raw materials are placed in a mixer for 3 minutes of mixing, and then placed in a twin-screw extruder for extrusion modification and granulation at 190° C. to obtain mixed granules.

[0073] S3: The obtained mixed particles are blown by a film blowing machine at a blowing temperature of 190° C. to obtain a fully biodegradable rice-specific mulch film.

[0074] Furthermore, the anti-hydrolysis agent includes monomeric carbodiimide and phenyl glycidyl ether, and the ratio of the two is 1:3. The antioxidant is antioxidant 168. The light stabilizer is polyoxyethylene (20) sorbitan monostearate and light stabilizer 119, and the ratio of the two is 1:20. The lubricant is erucic acid amide, and the opening agent is silicon dioxide micropowder.

[0075] Example 6

[0076] The method for preparing the fully biodegradable rice mulch film described in this embodiment comprises the following steps:

[0077] S1: Weigh 65% PBAT, 15% modified nano calcium carbonate, 5% PLA, 10% polytrimethylene terephthalate (PTT), 2% anti-hydrolysis agent, 1% antioxidant, 0.5% light stabilizer, 0.5% lubricant, and 1% anti-blocking agent by weight percentage.

[0078] The preparation method of the modified nano calcium carbonate is as follows: a certain amount of nano calcium carbonate is weighed and dispersed in anhydrous ethanol to obtain a suspension, alanine is dissolved in water, the suspension is added dropwise after heating for 1 hour, and after cross-linking reaction for 3 hours, the modified nano calcium carbonate is filtered, washed and dried to obtain the modified nano calcium carbonate.

[0079] S2: The weighed raw materials are placed in a mixer for 3 minutes of mixing, and then placed in a twin-screw extruder for extrusion modification and granulation at 190° C. to obtain mixed granules.

[0080] S3: The obtained mixed particles are blown by a film blowing machine at a blowing temperature of 190° C. to obtain a fully biodegradable rice-specific mulch film.

[0081] Furthermore, the anti-hydrolysis agent includes monomeric carbodiimide and phenyl glycidyl ether, and the ratio of the two is 1:3. The antioxidant is a combination of antioxidant 1010 and antioxidant 168, and the light stabilizer is polyoxyethylene (20) sorbitan monostearate and light stabilizer 622, and the ratio of the two is 1:20. The lubricant is stearic acid amide, and the anti-blocking agent is silicon dioxide micropowder.

[0082] The embodiments are preferred implementations of the present invention, but the present invention is not limited to the above-mentioned implementations. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essential content of the present invention belong to the protection scope of the present invention.

Claims

1. A method for preparing a fully biodegradable rice mulch film, characterized in that: The following steps are involved: S1: Weigh 50-65% of PBAT, 10-20% of modified nano calcium carbonate, 5-20% of PLA, 5-15% of polytrimethylene terephthalate (PTT), 0.2-2% of anti-hydrolysis agent, 0.2-2% of antioxidant, 0.2-2% of light stabilizer, 0.5-5% of lubricant and 1-5% of anti-blocking agent as raw materials by weight percentage; The preparation method of the modified nano calcium carbonate is as follows: weigh a certain amount of nano calcium carbonate and disperse it in anhydrous ethanol to obtain a suspension; dissolve the amino acid in water, heat it for 0.5 to 1 hour, add the suspension drop by drop, and after cross-linking reaction for 2 to 3 hours, filter, wash and dry to obtain the modified nano calcium carbonate; The anti-hydrolysis agent comprises monomeric carbodiimide and phenyl glycidyl ether, and the ratio of the two is 1:(1-5); S2: placing the weighed raw materials in a twin-screw extruder for extrusion modification and granulation to obtain mixed granules; S3: The mixed particles are blown by a film blowing machine to obtain a fully biodegradable rice-specific mulch film.

2. The preparation method according to claim 1, characterized in that: In step S1, the weight percentages of the PBAT, modified nano-calcium carbonate and PLA are 60-65%, 15-20% and 5-15% respectively; the ratio of monomeric carbodiimide and phenyl glycidyl ether in the hydrolysis resistance agent is 1:(1-3).

3. The preparation method according to claim 1, characterized in that: The heating temperature of the amino acid is 250-350°C.

4. The preparation method according to claim 1, characterized in that: The amino acids are one or more of lysine, arginine, histidine, alanine, glycine, valine, leucine, isoleucine, proline, phenylalanine, tryptophan, methionine, serine, threonine, cysteine, tyrosine, asparagine, glutamine and the like.

5. The preparation method according to claim 1, characterized in that: The antioxidant is one of antioxidant 1010 and antioxidant 168 or a combination of the two; the light stabilizer is polyoxyethylene (20) sorbitan monostearate and light stabilizer UV-783, light stabilizer 622 or light stabilizer 119, and the ratio of polyoxyethylene (20) sorbitan monostearate to light stabilizer UV-783, light stabilizer 622 or light stabilizer 119 is 1:(20-30); the lubricant is stearic acid amide or erucic acid amide, and the opening agent is silicon dioxide micropowder or erucic acid amide.

6. The preparation method according to claim 1, characterized in that: In step S2, before placing the raw materials in the twin-screw extruder, the raw materials are first placed in a mixer for mixing for 2 to 4 minutes.

7. The preparation method according to claim 1, characterized in that: In step S2, the granulation temperature is 150-200°C, preferably 180-200°C; in step S3, the blow molding temperature is 150-200°C, preferably 180-200°C.

8. The preparation method according to claim 1, characterized in that: The molding thickness of the fully biodegradable rice-specific mulch film is 0.05-0.01 mm.

9. A fully biodegradable rice mulch film prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the fully biodegradable rice-specific mulch film according to claim 9 in the field of crop planting.