All-steel radial tire belted layer cushion rubber material as well as preparation method and application of all-steel radial tire belted layer cushion rubber material
By using white carbon black, lauryl alcohol and silane coupling agent Si69 in the all-steel radial tire belt pad rubber material, the tensile strength and low fixed extension stress of the existing rubber material are solved. and the problem of high heat generation achieves high tensile strength, low heat generation and excellent mechanical properties, extending the service life of the tire.
Patent Information
- Application Number
- CN202410990036.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing all-steel radial tire belt layer pad glue materials have problems such as complex coordination system, low tensile strength and fixed extension stress and high heat generation.
The combination of white carbon black, lauryl alcohol and silane coupling agent Si69 and natural rubber and carbon black is used to modify white carbon black to improve its dispersion in the gel through the combined effect of silane coupling agent Si69 and lauryl alcohol. The dispersion of white carbon black is improved through nano-treatment, and a reinforcement is combined to improve the tensile strength of the glue and reduce heat generation.
The prepared rubber has high tensile strength, high fixed extension stress and low heat generation performance, which significantly improves the mechanical properties and service life of the tire belt layer and reduces the overall heat generation of the tire during use.
Smart Images

Figure BDA0004958603960000021 
Figure BDA0004958603960000081 
Figure FDA0004958603940000011
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber technology, and in particular to a rubber material used for cushioning rubber between different layers of a belt layer of an all-steel radial tire, a preparation method and an application thereof. Background Art
[0002] The belt layer is the main load-bearing component of the all-steel radial tire, and plays a key role in ensuring the tire has good durability, safety, handling, and multiple retreading performance.
[0003] Due to the high modulus of steel cord, the rubber compound is required to have a high tensile stress to reduce the shear deformation between the rubber compound and the cord. In addition, during the running of the tire, the deformation of the belt cushion rubber causes high heat generation in this area. As the tire running time increases, heat accumulation causes the belt cushion rubber area to have a high temperature, rubber aging and performance degradation, which in turn leads to tire belt rupture and tire scrapping. Therefore, the belt cushion rubber compound is also required to have low heat generation performance.
[0004] Currently, the rubber compound formula of the belt layer pad is mostly made of natural rubber and matched with a meta-acetic acid white system, but this formula still has problems such as a relatively complex matching system, low tensile strength and elongation stress, and high heat generation.
[0005] Therefore, there is an urgent need for a rubber compound for the belt layer of an all-steel radial tire with high tensile strength, high elongation stress, low heat generation and simple formula. Summary of the invention
[0006] The first purpose of the present invention is to provide a cushion rubber material for the belt layer of an all-steel radial tire. The second purpose of the present invention is to provide a method for preparing the cushion rubber material for the belt layer of an all-steel radial tire. The third purpose of the present invention is to provide an application of the cushion rubber material for the belt layer of an all-steel radial tire in the belt layer of an all-steel radial tire to solve the problems of complex matching system, low tensile strength and elongation stress, and high heat generation in the prior art.
[0007] In order to achieve the above objectives, the inventors provide the following technical solutions:
[0008] A full steel radial tire belt cushion rubber material, characterized in that it comprises the following components by weight:
[0009]
[0010] Natural rubber has the advantages of good processability and high strength of vulcanized rubber. It is suitable for the production of rubber for the belt layer of all-steel radial tires. The addition of carbon black can further improve the tensile strength, tear strength, tensile stress and wear resistance. Compared with carbon black, silica can effectively reduce the heat generation of the rubber. However, there are a large number of hydroxyl groups on the surface of silica, which can easily cause agglomeration between particles, resulting in strong polarity and hydrophilicity. It is difficult to disperse evenly in the rubber matrix, resulting in the heat generation and mechanical properties of the cushion rubber failing to reach the optimal level.
[0011] Therefore, the inventors thought of adding some modifiers to the formula to modify the silica to improve the dispersion performance of silica. Silane coupling agent Si69 modification is a widely used silica modification method. The sulfur-containing bifunctional silane coupling agent Si69 can effectively reduce the hydroxyl content on the surface of silica, thereby improving the dispersion of silica particles in the matrix. The sulfur-containing functional group can also participate in the vulcanization of rubber, so that a covalent connection is formed between the silica and rubber molecular chains, thereby enhancing the bonding force between the filler and the matrix natural rubber.
[0012] However, the inventors found that adding silane coupling agent Si69 to the formula had limited effect on changing the hydrophilicity of silica, resulting in limited improvement in the heat generation performance of the finally prepared all-steel radial tire belt cushion rubber compound.
[0013] The inventors found that lauryl alcohol can also change the hydrophilicity of silica. Lauryl alcohol undergoes dehydration condensation with the hydroxyl groups of silica and is grafted onto silica. Lauryl alcohol has a relatively long chain length and can shield part of the hydroxyl groups on the surface of silica by winding and other means. The addition of lauryl alcohol greatly improves the dispersibility of silica in the rubber compound. However, the added lauryl alcohol affects the mechanical properties of the prepared all-steel radial tire belt and cushion rubber compound, resulting in lower mechanical performance parameters such as tensile strength, tear strength, tensile stress at break, and the like of the finally prepared all-steel radial tire belt and cushion rubber compound.
[0014] The inventor innovatively added silane coupling agent Si69 and lauryl alcohol to the formula and found that the combination of silane coupling agent Si69 and lauryl alcohol in the formula had excellent effect on improving the thermal performance of the all-steel radial tire belt cushion rubber material, and the prepared all-steel radial tire belt cushion rubber material had excellent mechanical properties.
[0015] The inventors further discovered that when silane coupling agent Si69 and lauryl alcohol are added in a ratio of 1:2 in the formula, the thermal performance and mechanical properties of the all-steel radial tire belt cushion rubber are the best.
[0016] The active groups bonded to the surface of the reinforcing agent can combine with the rubber matrix molecules to maintain the tensile strength of the rubber and reduce heat generation. Adding reinforcing agents to the formula can further reduce the heat generation of the rubber while ensuring that the rubber has a high tensile strength.
[0017] Furthermore, the white carbon black is nano-sized white carbon black that has been subjected to nano-processing.
[0018] After ultrafine nano-processing, the specific surface area of white carbon black increases, the active groups increase, the dispersibility in the rubber compound is improved, and the interaction between the white carbon black and the natural rubber molecules is strengthened.
[0019] Furthermore, the white carbon black is white carbon black 955.
[0020] Furthermore, the carbon black is carbon black N326.
[0021] Furthermore, the antioxidant is one or more of antioxidant A, antioxidant D, antioxidant RD, antioxidant 246, antioxidant 4010, antioxidant SP, and antioxidant WH-02.
[0022] The present invention also provides a method for preparing a cushion rubber material for a belt layer of an all-steel radial tire as described in the above technical solution, comprising the following steps:
[0023] S1: kneading natural rubber, zinc oxide, carbon black, white carbon black, lauryl alcohol, silane coupling agent Si69, antioxidant and reinforcing agent to obtain a masterbatch;
[0024] S2 performs two-stage refining on the first-stage masterbatch to obtain the second-stage mixed rubber;
[0025] S3 adds sulfur and other additives, and performs three-stage mixing on the two-stage rubber vulcanization to obtain the belt layer cushion rubber.
[0026] Furthermore, the first stage mixing and the second stage mixing are carried out in a BB430 type internal mixer, and the third stage mixing is carried out in a GK255 type internal mixer.
[0027] Furthermore, the mixing temperature of the first stage mixing and the second stage mixing is 145-160°C, and the temperature of the third stage mixing is 95-105°C.
[0028] Furthermore, the first-stage masterbatch must be left at room temperature for at least 8 hours before entering the next step, and the second-stage rubber must be left at room temperature for at least 8 hours before entering the next step.
[0029] The present invention also provides an application of the all-steel radial tire belt cushion rubber material described in the above technical solution in the all-steel radial tire belt.
[0030] Compared with the prior art, the present invention has the following advantages and effects:
[0031] (1) The present application uses white carbon black, lauryl alcohol, silane coupling agent Si69 in combination with natural rubber and carbon black to prepare a full-steel radial tire belt layer rubber material with high tensile strength, high tensile stress and low heat generation performance. The prepared rubber material is used between different layers of the tire belt layer to provide better support for the end points of the belt layer, thereby making the different layers of the tire belt layer have obvious strain, better matching the stress distribution between different layers of the tire belt layer, reducing the shear deformation caused by the belt layer being subjected to force during the use of the tire, reducing the overall heat generation of the tire during use, and improving the service life of the tire.
[0032] (2) The formula of the present application does not use other functional synthetic rubbers, but only uses a single natural rubber to ensure the tensile strength and processing performance of the rubber compound. The raw materials are simple, the cost is low, and the economic effect is good. Specific embodiments
[0033] Example 1
[0034] 1.1 Raw materials
[0035] 100 parts of natural rubber, 8 parts of zinc oxide, 45 parts of carbon black, 9 parts of white carbon black, 8 parts of lauryl alcohol, 4 parts of silane coupling agent Si69, 8 parts of hardening and reinforcing agent 8180, 2.8 parts of antioxidant 246, 15.2 parts of sulfur and other additives.
[0036] 1.2 Preparation
[0037] S1: natural rubber, zinc oxide, carbon black, white carbon black, lauryl alcohol, silane coupling agent Si69, antioxidant and reinforcing agent are mixed in a BB430 type internal mixer at a mixing temperature of 155°C and a mixing time of 120s to obtain a masterbatch;
[0038] S2: The first-stage masterbatch is subjected to second-stage refining in a BB430 internal mixer, with a refining time of 85 seconds and a refining temperature of 155°C to obtain a second-stage rubber mixture;
[0039] S3 adds sulfur and other additives, and performs three-stage mixing on the two-stage rubber vulcanization, with a vulcanization time of 75 seconds and a vulcanization temperature of 100° C. to obtain the belt layer cushion rubber.
[0040] Example 2
[0041] 1.1 Raw materials
[0042] 100 parts of natural rubber, 6 parts of zinc oxide, 40 parts of carbon black, 8 parts of white carbon black, 5 parts of lauryl alcohol, 3 parts of silane coupling agent Si69, 6 parts of hardening and reinforcing agent 8180, 2.5 parts of antioxidant 246, 12.5 parts of sulfur and other additives.
[0043] 1.2 Preparation
[0044] S1: natural rubber, zinc oxide, carbon black, white carbon black, lauryl alcohol, silane coupling agent Si69, antioxidant and reinforcing agent are mixed in a BB430 type internal mixer at a mixing temperature of 155°C and a mixing time of 120s to obtain a masterbatch;
[0045] S2: The first-stage masterbatch is subjected to second-stage refining in a BB430 internal mixer, with a refining time of 85 seconds and a refining temperature of 155°C to obtain a second-stage rubber mixture;
[0046] S3 adds sulfur and other additives, and performs three-stage mixing on the two-stage rubber vulcanization, with a vulcanization time of 75 seconds and a vulcanization temperature of 100° C. to obtain the belt layer cushion rubber.
[0047] Example 3
[0048] 1.1 Raw materials
[0049] 100 parts of natural rubber, 10 parts of zinc oxide, 48 parts of carbon black, 12 parts of white carbon black, 10 parts of lauryl alcohol, 4.5 parts of silane coupling agent Si69, 10 parts of hardening and reinforcing agent 8180, 3.5 parts of antioxidant 246, 18 parts of sulfur and other additives.
[0050] 1.2 Preparation
[0051] S1: natural rubber, zinc oxide, carbon black, white carbon black, lauryl alcohol, silane coupling agent Si69, antioxidant and reinforcing agent are mixed in a BB430 type internal mixer at a mixing temperature of 155°C and a mixing time of 120s to obtain a masterbatch;
[0052] S2: The first-stage masterbatch is subjected to second-stage refining in a BB430 internal mixer, with a refining time of 85 seconds and a refining temperature of 155°C to obtain a second-stage rubber mixture;
[0053] S3 adds sulfur and other additives, and performs three-stage mixing on the two-stage rubber vulcanization, with a vulcanization time of 75 seconds and a vulcanization temperature of 100° C. to obtain the belt layer cushion rubber.
[0054] Comparative Example 1
[0055] The raw materials and preparation were carried out according to Example 1, except that white carbon black, lauryl alcohol and silane coupling agent Si69 were not added.
[0056] Comparative Example 2
[0057] The raw materials and preparation were carried out according to Example 1, except that lauryl alcohol and silane coupling agent Si69 were not added.
[0058] Comparative Example 3
[0059] The raw materials and preparation were carried out according to Example 1, except that lauryl alcohol was not added.
[0060] Comparative Example 4
[0061] The raw materials and preparation were carried out according to Example 1, except that the silane coupling agent Si69 was not added.
[0062] Test example
[0063] The belt layer cushion rubbers obtained in the above Examples 1 to 3 and Comparative Examples 1-2 were subjected to performance tests, and the results are shown in Table 1.
[0064] Table 1 Test data of Examples 1-3 and Comparative Examples 1-2
[0065]
[0066] As can be seen from the table, from Comparative Examples 1 and 2, adding white carbon black to the system containing natural rubber and carbon black in Comparative Example 2 can improve the heat generation performance of the rubber compound. However, if only white carbon black is added, due to the presence of a large number of hydroxyl groups on the surface of white carbon black, it is easy to cause agglomeration between particles, and it is difficult to disperse evenly in the rubber matrix, resulting in the heat generation and mechanical properties of the rubber compound in Comparative Example 2 not reaching the optimal level, and its loss factor tanδ@60℃ and compression heat generation value are both relatively high.
[0067] In Comparative Example 3, only silane coupling agent Si69 and white carbon black were added, and no lauryl alcohol was added. The mechanical properties such as tensile stress, tensile strength and tensile elongation at break were improved to a certain extent compared with those in Comparative Example 1. However, the loss factor tanδ@60℃ and the compression heat generation value were still relatively high compared with those in Example 1 in which white carbon black, silane coupling agent Si69 and lauryl alcohol were used in combination, and the improvement in heat generation performance was limited. This may be because the silane coupling agent Si69 is easily hydrolyzed, and a condensation reaction will occur after hydrolysis, which leads to a weakened reaction ability to the hydroxyl groups on the surface of white carbon black, greatly reducing the modification efficiency, and having a limited effect on changing the hydrophilicity of white carbon black.
[0068] In Comparative Example 4, only lauryl alcohol and white carbon black were added, and no silane coupling agent Si69 was added. The heat generation performance was improved excellently. This is because lauryl alcohol can greatly enhance the dispersibility of white carbon black. However, the addition of lauryl alcohol will affect the mechanical properties of the rubber, resulting in lower mechanical parameters such as tensile stress, tensile strength and elongation at break of the prepared rubber.
[0069] White carbon black, lauryl alcohol and silane coupling agent Si69 were added to the formulation system of Examples 1-3, and the prepared rubber had low loss factor tanδ@60°C and compression heat generation value, high mechanical parameter values such as tensile stress, tensile strength and tensile elongation, and had excellent heat generation and mechanical properties.
[0070] Therefore, only by using white carbon black, lauryl alcohol, silane coupling agent Si69 in combination with natural rubber and carbon black can the all-steel radial tire belt layer cushion rubber compound with excellent heat generation and mechanical properties be obtained.
Claims
1. A rubber material for the belt layer of an all-steel radial tire, characterized by: By weight, it includes the following components:
2. The all-steel radial tire belt cushion rubber material according to claim 1, characterized in that: The white carbon black is nano-sized white carbon black that has been subjected to nano-processing.
3. The all-steel radial tire belt cushion rubber material according to claim 2, characterized in that: The white carbon black is white carbon black 955.
4. The all-steel radial tire belt cushion rubber material according to any one of claims 1 to 3, characterized in that: The carbon black is carbon black N326.
5. The all-steel radial tire belt cushion rubber material according to any one of claims 1 to 3, characterized in that: The antioxidant is one or more of antioxidant A, antioxidant D, antioxidant RD, antioxidant 246, antioxidant 4010, antioxidant SP, and antioxidant WH-02.
6. The all-steel radial tire belt cushion rubber material according to any one of claims 1 to 3, characterized in that: The reinforcing agent is one or more of the hardening reinforcing agent 8180 and the hardening reinforcing agent 9010.
7. A method for preparing a cushion rubber compound for a belt layer of an all-steel radial tire according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: kneading natural rubber, zinc oxide, carbon black, white carbon black, lauryl alcohol, silane coupling agent Si69, antioxidant and reinforcing agent to obtain a masterbatch; S2 performs two-stage refining on the first-stage masterbatch to obtain the second-stage mixed rubber; S3 adds sulfur and other additives, and performs three-stage mixing on the two-stage rubber vulcanization to obtain the belt layer cushion rubber material.
8. A method for preparing a cushion rubber compound for a belt layer of an all-steel radial tire according to claim 7, characterized in that: The mixing temperature of the first stage mixing and the second stage mixing is 145-160°C, and the temperature of the third stage mixing is 95-105°C.
9. A method for preparing a cushion rubber compound for a belt layer of an all-steel radial tire according to claim 8, characterized in that: The first stage masterbatch must be left at room temperature for at least 8 hours before entering the next step, and the second stage rubber must be left at room temperature for at least 8 hours before entering the next step.
10. Use of the all-steel radial tire belt cushion rubber material according to any one of claims 1 to 6 between the belt layers of the all-steel radial tire.