Medical antibacterial nanometer butyronitrile glove and preparation method thereof

By using antibacterial composite nitrile rubber and chlorinated butyl rubber in medical gloves and adding microcapsule nanoenhancing agents, the problems of uneven distribution of inorganic fillers and insufficient antibacterial performance are solved, and the mechanical properties and antibacterial effects of gloves are significantly improved. .

CN118930992AActive Publication Date: 2024-11-12SHANGHAI HEHAO MEDICAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411077865.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

In the prior art, when mixing different kinds of rubbers such as nitrile rubber to prepare medical gloves, the added inorganic filler is unevenly distributed in the rubber matrix, resulting in the reduction of the elongation and tensile strength of the prepared medical gloves, and insufficient antibacterial performance. .

Method used

Antibacterial composite nitrile rubber and chlorinated butyl rubber are used as base materials, microcapsule nanointensifiers are added, and the mechanical and antibacterial properties of the gloves are improved by modifying the design of antibacterial agents and additives. The specific method includes reacting cinnamic acid with tripercyanochloride to form an ester compound, performing polypolytic reaction, and preparing nano-scale microcapsule enhancer by spray drying, combining anti-aging additives and plasticizers, and performing vulcanization molding.

Benefits of technology

It significantly improves the tensile strength, elongation and hardness of medical antibacterial nanonitrile gloves, enhances antibacterial properties, and improves the overall mechanical properties and heat resistance of the gloves.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004982868680000031
    Figure BDA0004982868680000031
  • Figure BDA0004982868680000041
    Figure BDA0004982868680000041
  • Figure BDA0004982868680000131
    Figure BDA0004982868680000131
Patent Text Reader

Abstract

The invention discloses a medical antibacterial nano butyronitrile glove and a preparation method thereof, belongs to the technical field of medical gloves, and is used for solving the technical problems of poor mechanical strength and poor antibacterial property when the medical gloves are prepared by blending nitrile rubber and other rubber materials in the prior art. The composite spherical particle comprises antibacterial composite nitrile rubber, chlorinated butyl rubber, a microcapsule nano reinforcing agent, an anti-aging auxiliary agent, a vulcanizing auxiliary agent and a plasticizer, inorganic materials are ground into different particle sizes and divided into mother particles and child particles, the mother particles and the child particles are processed through a micro-nano particle composite system, and composite spherical particles with inner and outer layer structures are obtained. The composite spherical particles are coated with a wall material, a microcapsule nano reinforcing agent is prepared, cyanuric chloride enriches cinnamic acid and then is compounded with nitrile rubber, so that the antibacterial property of the nitrile rubber is improved, and the prepared medical antibacterial nano butyronitrile gloves have excellent mechanical property and antibacterial property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical gloves, and in particular to a medical antibacterial nano-nitrile glove and a preparation method thereof. Background Art

[0002] Rubber is a general term for all polymer elastomers. It is formed into a three-dimensional network polymer material through a vulcanization process by chemically cross-linking linear polymer materials. That is, various raw rubber compounds are converted into vulcanized rubber. As a highly elastic polymer material, rubber has excellent air permeability, resistance to various chemical media and electrical insulation properties. These properties make rubber an irreplaceable and important industrial material among polymer materials, such as various tires, wires and cables, hoses, medical gloves and sealing rubber accessories.

[0003] In addition, rubber can be used, blended, and compounded with a variety of materials to modify it and obtain good comprehensive performance. For example, its mechanical properties can be improved by adding inorganic materials and blending different types of rubber.

[0004] Patent application CN103554565A discloses a medical glove blended with natural rubber and nitrile rubber and a preparation method thereof, wherein natural rubber latex, nitrile rubber latex, a stabilizer, sulfur, zinc oxide, titanium dioxide and an alkaline filler are mixed to prepare a medical glove blended with natural rubber and nitrile rubber; however, the alkaline filler has an uneven distribution problem in the rubber matrix, which impairs the mechanical properties of the prepared medical gloves, such as elongation at break and tensile strength, while improving the mechanical strength of the prepared medical gloves. In addition, the medical gloves themselves need to have certain antibacterial properties.

[0005] Patent application CN112812261A discloses a method for preparing a water-based polyurethane emulsion and a nitrile rubber-polyurethane composite gloves, wherein the water-based polyurethane emulsion is a cationic antibacterial water-based polyurethane, and phenolic acid is introduced into the water-based polyurethane to form a quaternary ammonium salt structure, so as to improve the antibacterial effect of the prepared composite gloves; however, the compatibility of the two basic materials between the water-based polyurethane emulsion and the nitrile rubber is improved only through hydrogen bonds and electrostatic interactions between anions and cations, and the integrity of the prepared gloves cannot be improved, that is, the mechanical properties of the prepared composite gloves cannot be improved. Therefore, how to prepare a rubber glove with excellent mechanical properties and antibacterial properties is still a technical problem that needs to be solved urgently, and a solution is now proposed to address the technical defects in this regard. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing medical antibacterial nano-nitrile gloves, which is used to solve the problem in the prior art that when different types of rubber such as nitrile rubber are blended to prepare medical gloves, the added inorganic filler is unevenly distributed in the rubber matrix, thereby reducing the elongation at break and tensile strength of the prepared medical gloves. In addition, the antibacterial property of medical gloves is also a technical problem that needs to be solved urgently.

[0007] The purpose of the present invention can be achieved through the following technical scheme: a medical antibacterial nano-nitrile glove, comprising the following components in parts by weight: 60-80 parts of antibacterial composite nitrile rubber, 20-40 parts of chlorinated butyl rubber, 5-10 parts of microcapsule nano-enhancer, 2-3 parts of anti-aging aid, 2-5 parts of vulcanization aid and 5-10 parts of plasticizer.

[0008] Furthermore, the preparation method of the antibacterial composite nitrile rubber comprises the following steps:

[0009] S1. Mix cinnamic acid, cyanuric chloride, sodium carbonate and ethanol evenly to obtain a premix; react the premix at 50-60°C for 2-3h, then heat to 70-75°C, and react at this temperature for 2-3h; then heat to 80-90°C, evaporate the ethanol solvent, and obtain a solid modified antibacterial agent;

[0010] With ethanol as solvent and sodium carbonate as nucleophilic reagent, the carboxyl group in cinnamic acid and the chloride ion in cyanuric chloride undergo nucleophilic substitution reaction to generate corresponding esters, which is the prepared modified antibacterial agent.

[0011] The reaction equation of cinnamic acid and cyanuric chloride is as follows:

[0012]

[0013] S2, adding the modified antibacterial agent and the nitrile rubber to a two-roll mill and uniformly dispersing them to obtain a mixture; adding the mixture to a double-roll mill for plasticizing to obtain an antibacterial composite nitrile rubber.

[0014] The modified antimicrobial agent and the nitrile rubber are physically and uniformly dispersed in a two-roll mill in advance to obtain a mixture. Under high temperature conditions, due to the presence of unsaturated double bonds in both the modified antimicrobial agent and the nitrile rubber, an addition polymerization reaction occurs to prepare an antimicrobial composite nitrile rubber.

[0015] Furthermore, in step S1, the dosage ratio of cinnamic acid, cyanuric chloride, sodium carbonate and ethanol is 50-60g:18g:5g:250mL; in step S2, the dosage ratio of modified antibacterial agent and nitrile rubber is 1-5g:50g, the plasticizing temperature is 120-150°C, and the plasticizing time is 5-10min.

[0016] Furthermore, the preparation method of the microcapsule nano-enhancer comprises the following steps:

[0017] A1. Grinding heavy calcium carbonate to 300-500 μm to obtain mother particles; grinding wollastonite and dolomite to 30-50 μm to obtain daughter particles; adding the mother particles and daughter particles to a micro-nano particle composite system, performing composite and spherical treatments to obtain composite spherical particles;

[0018] Heavy calcium carbonate is used as the mother particle, and a mixture of wollastonite and dolomite is used as the daughter particle. The mother particle and the daughter particle are ground to a diameter ratio of 10:1. The mother particle and the daughter particle are then added into a micro-nano particle composite system to prepare composite spherical particles.

[0019] A2, methanol and trichlorocyanuric acid silicon react at 20-30°C for 2-3h to obtain a product; the product is split and a fraction of polymethoxysilane is intercepted;

[0020] Methanol and trichlorosilane undergo alcoholysis to prepare polymethoxysilanes containing different numbers of methoxy groups.

[0021] The reaction equation of methanol and trichlorosilane is as follows:

[0022]

[0023] A3, gelatin and deionized water are mixed, heated and stirred until completely dissolved; then casein and polymethoxysilane are added to obtain a mixed liquid; 1 mol / L NaOH solution is added dropwise to the mixed liquid to adjust the pH value of the mixed liquid to 8-9, so that the casein is completely dissolved, first reacted at 80-90°C for 2-3h, and then allowed to stand at room temperature for 24h to obtain a wall material solution;

[0024] Gelatin and casein are used as the wall materials of the prepared microcapsule nano-enhancer; wherein, polymethoxysilane undergoes a hydrolysis reaction in the wall material solution to obtain silanol, and the silanol can undergo an esterification reaction with the carboxyl group of the amino acid in gelatin and casein, and then stand for a period of time to obtain a wall material solution modified by a coupling agent.

[0025] S4. Add the composite spherical particles into the wall material solution, then adjust the pH value of the wall material solution to 2-3 with 1 mol / L citric acid, and adopt spray drying to prepare a nano-scale microcapsule enhancer.

[0026] The invention adopts a spray drying method, uses composite spherical particles as core materials, and coats the composite spherical particles with wall materials to prepare a nano-scale microcapsule reinforcing agent.

[0027] Furthermore, in step A1, the ratio of wollastonite to dolomite is 1:1, and the ratio of mother particles to daughter particles is 2:1, based on parts by weight; the rotor speed of the PCS system is 2000-3000 r / min, and the processing time is 10-20 min.

[0028] Furthermore, in step A2, the usage ratio of methanol and trichlorocyanuric acid silicon is 96g:100-135g; in step A3, the usage ratio of gelatin, deionized water, casein and polymethoxysilane is 15g:300mL:5g:10-20g; in step A4, the usage ratio of composite spherical particles and wall material solution is 50-60g:100mL.

[0029] As another aspect of the present invention, a method for preparing medical antibacterial nano-nitrile gloves comprises the following steps:

[0030] B1, adding the antibacterial composite nitrile rubber and chlorinated butyl rubber into an open mill for mixing, and then sequentially adding an anti-aging agent, a vulcanizing agent and a plasticizer, and under the shearing action of a double roller, each component is in a cutting and mixing state to obtain a vulcanized rubber material;

[0031] B2. Add the vulcanized rubber material into the mold, press-form it in a high-temperature vulcanizer, then take out the mold, cool it to room temperature, and demould it to obtain the antibacterial composite nitrile rubber.

[0032] Further, in step B1, the amount ratio of the antibacterial composite nitrile rubber, chlorinated butyl rubber, antioxidant, vulcanization aid and plasticizer is 60-80:20-40:2-3:2-5:5-10 in parts by weight; the antioxidant includes 10 parts of naphthylamine antioxidant and 10 parts of ketoamine antioxidant in parts by weight, and the naphthylamine antioxidant is any one of antioxidant A, antioxidant MB and antioxidant NDPA; the ketoamine antioxidant includes any one of antioxidant RD and antioxidant BLE; the vulcanization aid includes 2-5 parts of sulfur, 0.5 parts of vulcanization accelerator and 0.5 parts of vulcanization activator in parts by weight; the plasticizer is any one of black ointment, white ointment or castor oil.

[0033] Furthermore, in step B2, the vulcanization temperature is 200° C. and the vulcanization time is 3-5 min.

[0034] The medical antibacterial nano-nitrile gloves prepared by the invention include antibacterial composite nitrile rubber and chlorinated butyl rubber as main materials, and the added auxiliary agents include anti-aging auxiliary agents, vulcanization auxiliary agents and plasticizers, wherein the vulcanization auxiliary agents include sulfur, vulcanization accelerators and vulcanization activators.

[0035] The present invention has the following beneficial effects:

[0036] 1. The medical antibacterial nano-nitrile gloves prepared by the present invention use nitrile rubber and chlorobutyl rubber as base materials, and add microcapsule nano-enhancers to improve their mechanical properties; the microcapsule nano-enhancer uses composite spherical particles as core materials, and gelatin, casein and polymethoxysilane as wall material components; the inorganic material is ground to the nanoscale, which can enhance its own mechanical properties and is beneficial for uniform dispersion in the basic rubber material. In order to avoid the agglomeration of inorganic materials with tiny particle sizes in the rubber base material, the present invention prepares the inorganic material into microcapsules; the inorganic material is divided into mother particles and daughter particles according to the different grinding particle sizes, and is processed by a micro-nano particle composite system to obtain composite spherical particles with inner and outer layers and dense structure. Since polymethoxysilane can react with gelatin and casein, the compactness of the wall material is improved; the present invention adopts a spray drying method to disperse the core material in the wall material solution. During the spray drying process, the hot air flow will quickly evaporate the water in the droplets, and the wall material will form a mesh structure that can shield the core material particles and allow the water to evaporate from it, forming a dense vitreous structure. The present invention can significantly improve the tensile strength, elongation at break, hardness and other mechanical properties of the prepared medical antibacterial nano nitrile gloves by adding microcapsule nano enhancers.

[0037] 2. The present invention pre-modifies the nitrile rubber for antibacterial properties; uses cyanuric chloride as a carrier to enrich the antibacterial substance cinnamic acid, thereby obtaining a modified antibacterial agent with improved antibacterial efficiency; both the nitrile rubber and the modified antibacterial agent contain unsaturated double bonds, which are plasticized under high temperature conditions and subjected to addition reaction, thereby preparing an antibacterial composite nitrile rubber grafted with the modified antibacterial agent. The antibacterial composite nitrile rubber and chlorobutyl rubber are mixed and poly-added to obtain a vulcanized rubber material; the double bonds in the antibacterial composite nitrile rubber and chlorobutyl rubber are further added to increase the structural saturation, thereby further improving the heat resistance and aging resistance of the vulcanized rubber material itself. The present invention designs the ratio of anti-aging aids, vulcanization aids and plasticizer-related aids to prepare a medical antibacterial nano-nitrile rubber with excellent mechanical properties and strong antibacterial properties. DETAILED DESCRIPTION

[0038] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] This embodiment provides a method for preparing a microcapsule nano-enhancer for medical antibacterial nano-nitrile gloves, comprising the following steps:

[0041] A1. Add heavy calcium carbonate to a planetary ball mill for grinding, grind the heavy calcium carbonate to a particle size of 300 μm to obtain mother particles; add 10 parts of wollastonite and 10 parts of dolomite to a planetary ball mill by weight, grind the particle size to 30 μm to obtain daughter particles; put 20 parts of mother particles and 10 parts of daughter particles into a micro-nano particle composite system by weight, composite and spherical the mother particles and daughter particles to obtain composite spherical particles. The micro-nano particle composite system uses argon as a protective gas, the rotor speed of the system is 2000 r / min, and the processing time of the system is 10 min.

[0042] A2, a 500mL three-necked flask was connected to a condenser and an electromagnetic stirrer respectively, 96g of methanol and 100g of trichlorosilane were added to the three-necked flask, cooling medium water was passed into the condenser, and then the three-necked flask was heated to 20°C and reacted for 2h to obtain the product; the product was fractionated to intercept the fraction of the target product polymethoxysilane.

[0043] A3. Add 15 g of gelatin and 300 mL of deionized water into a 500 mL beaker, heat and stir the beaker until the gelatin is completely dissolved, then add 5 g of casein and 10 g of polymethoxysilane to obtain a mixed solid-liquid; then adjust the pH value of the mixed solid-liquid to 8 with a 1 mol / L NaOH solution to completely dissolve the casein, first react at 80-90°C for 2-3 hours, then stand at room temperature for 24 hours to obtain a wall material solution;

[0044] A4. Add 50 g of composite spherical particles to 100 mL of wall material solution, adjust the pH value of the wall material solution to 2 with 1 mol / L citric acid, and prepare microcapsule nano-enhancer by spray drying. During the spray drying process, the inlet air temperature is 120 ° C, the feed rate is 15 mL / min, and the inlet air volume is 1m 3 / min.

[0045] Example 2

[0046] This embodiment provides a method for preparing a microcapsule nano-enhancer for medical antibacterial nano-nitrile gloves, comprising the following steps:

[0047] A1. Add heavy calcium carbonate to a planetary ball mill for grinding, grind the heavy calcium carbonate to a particle size of 400 μm to obtain mother particles; add 10 parts of wollastonite and 10 parts of dolomite to a planetary ball mill by weight, grind the particle size to 40 μm to obtain daughter particles; add 20 parts of mother particles and 10 parts of daughter particles to a micro-nano particle composite system by weight, composite and spherical the mother particles and daughter particles to obtain composite spherical particles. The micro-nano particle composite system uses argon as a protective gas, the rotor speed of the system is 2500 r / min, and the processing time of the system is 15 min.

[0048] A2, a 500mL three-necked flask was connected to a condenser and an electromagnetic stirrer respectively, 96g of methanol and 115g of trichlorosilane were added to the three-necked flask, cooling medium water was passed into the condenser, and then the three-necked flask was heated to 25°C and reacted for 2.5h to obtain the product; the product was fractionated to intercept the fraction of the target product polymethoxysilane.

[0049] A3. Add 15 g of gelatin and 300 mL of deionized water into a 500 mL beaker, heat and stir the beaker until the gelatin is completely dissolved, then add 5 g of casein and 15 g of polymethoxysilane to obtain a mixed solid-liquid; then adjust the pH value of the mixed solid-liquid to 8.3 with a 1 mol / L NaOH solution to completely dissolve the casein, first react at 80-90°C for 2-3 hours, then stand at room temperature for 24 hours to obtain a wall material solution;

[0050] A4. Add 53 g of composite spherical particles to 100 mL of wall material solution, adjust the pH value of the wall material solution to 2.5 with 1 mol / L citric acid, and prepare microcapsule nano-enhancer by spray drying. During the spray drying process, the inlet air temperature was 125 °C, the feed rate was 15 mL / min, and the inlet air volume was 2 m 3 / min.

[0051] Example 3

[0052] This embodiment provides a method for preparing a microcapsule nano-enhancer for medical antibacterial nano-nitrile gloves, comprising the following steps:

[0053] A1. Add heavy calcium carbonate to a planetary ball mill for grinding, grind the heavy calcium carbonate to a particle size of 500 μm to obtain mother particles; add 10 parts of wollastonite and 10 parts of dolomite to a planetary ball mill by weight, grind the particle size to 50 μm to obtain daughter particles; add 20 parts of mother particles and 10 parts of daughter particles to a micro-nano particle composite system by weight, composite and spherical the mother particles and daughter particles to obtain composite spherical particles. Among them, the micro-nano particle composite system uses argon as a protective gas, the rotor speed of the system is 3000 r / min, and the processing time of the system is 20 minutes.

[0054] A2, a 500mL three-necked flask was connected to a condenser and an electromagnetic stirrer respectively, 96g of methanol and 135g of trichlorosilane were added to the three-necked flask, cooling medium water was passed into the condenser, and then the three-necked flask was heated to 30°C and reacted for 3h to obtain the product; the product was fractionated to intercept the fraction of the target product polymethoxysilane.

[0055] A3. Add 15 g of gelatin and 300 mL of deionized water into a 500 mL beaker, heat and stir the beaker until the gelatin is completely dissolved, then add 5 g of casein and 20 g of polymethoxysilane to obtain a mixed solid-liquid; then adjust the pH value of the mixed solid-liquid to 9 with a 1 mol / L NaOH solution to completely dissolve the casein, first react at 90° C. for 3 h, then stand at room temperature for 24 h to obtain a wall material solution;

[0056] A4. Add 60 g of composite spherical particles to 100 mL of wall material solution, adjust the pH value of the wall material solution to 3 with 1 mol / L citric acid, and prepare microcapsule nano-enhancer by spray drying. During the spray drying process, the inlet air temperature was 130 °C, the feed rate was 15 mL / min, and the inlet air volume was 3 m 3 / min.

[0057] Example 4

[0058] This embodiment provides a method for preparing an antibacterial composite nitrile rubber for medical antibacterial nano-nitrile gloves, comprising the following steps:

[0059] S1. Add 50g of cinnamic acid, 18g of cyanuric chloride, 5g of sodium carbonate and 250mL of ethanol into a 500mL three-necked flask, connect one end of the three-necked flask to a stirrer, one end to a thermometer and one end to a seal, stir at room temperature at 100r / min for 5min to obtain a premix; then transfer the three-necked flask to a water bath, react at 50°C for 2h, then heat to 70°C, react at this temperature for 2h, then heat to 80°C, evaporate the ethanol solvent to obtain a solid, which is the modified antibacterial agent.

[0060] S2. Mix 1 g of the modified antibacterial agent and 50 g of nitrile rubber, and evenly disperse them in a two-roll mill to obtain a mixture; add the mixture to a two-roll mill, and plasticize at 120° C. for 5 min to obtain an antibacterial composite nitrile rubber.

[0061] Example 5

[0062] This embodiment provides a method for preparing an antibacterial composite nitrile rubber for medical antibacterial nano-nitrile gloves, comprising the following steps:

[0063] S1. Add 53g of cinnamic acid, 18g of cyanuric chloride, 5g of sodium carbonate and 250mL of ethanol into a 500mL three-necked flask, connect one end of the three-necked flask to a stirrer, one end to a thermometer and one end to a seal, stir at room temperature at 150r / min for 6min to obtain a premix; then transfer the three-necked flask to a water bath, react at 55°C for 2.5h, then heat to 72°C, react at this temperature for 2.5h, then heat to 85°C, evaporate the ethanol solvent to obtain a solid, which is the modified antibacterial agent.

[0064] S2. Mix 2 g of the modified antibacterial agent and 50 g of nitrile rubber, and evenly disperse them in a two-roll mill to obtain a mixture; add the mixture to a two-roll mill, and plasticize at 135° C. for 8 min to obtain an antibacterial composite nitrile rubber.

[0065] Example 6

[0066] This embodiment provides a method for preparing an antibacterial composite nitrile rubber for medical antibacterial nano-nitrile gloves, comprising the following steps:

[0067] S1. Add 60g of cinnamic acid, 18g of cyanuric chloride, 5g of sodium carbonate and 250mL of ethanol into a 500mL three-necked flask, connect one end of the three-necked flask to a stirrer, one end to a thermometer and one end to a seal, stir at room temperature at 200r / min for 10min to obtain a premix; then transfer the three-necked flask to a water bath, react at 60°C for 3h, then heat to 75°C, react at this temperature for 3h, then heat to 90°C, evaporate the ethanol solvent to obtain a solid, which is the modified antibacterial agent.

[0068] S2. Mix 5 g of the modified antibacterial agent and 50 g of nitrile rubber, and evenly disperse them in a two-roll mill to obtain a mixture; add the mixture to a two-roll mill, and plasticize at 150° C. for 10 min to obtain an antibacterial composite nitrile rubber.

[0069] Example 7

[0070] This embodiment provides a method for preparing medical antibacterial nano-nitrile gloves, comprising the following steps:

[0071] B1. According to parts by weight, 60 parts of the antibacterial composite nitrile rubber prepared in Example 4 and 20 parts of chlorinated butyl rubber are added to an open mill and mixed for 4 minutes, and then 5 parts of the microcapsule nano-enhancer prepared in Example 1, 1 part of antioxidant A, 1 part of antioxidant RD, 1 part of sulfur, 0.25 parts of vulcanization accelerator monothiuram sulfide, 0.25 parts of vulcanization activator monothiuram sulfide and 5 parts of black ointment are added in sequence, and mixed uniformly to obtain a vulcanized rubber material.

[0072] B2. Add the vulcanized rubber material into the mold, pressurize and mold it in a high-temperature vulcanizer at 200° C. for 3 minutes; then take out the mold, cool it to room temperature, and demold it to obtain the antibacterial composite nitrile rubber.

[0073] Example 8

[0074] This embodiment provides a method for preparing medical antibacterial nano-nitrile gloves, comprising the following steps:

[0075] B1. According to parts by weight, 70 parts of the antibacterial composite nitrile rubber prepared in Example 5 and 30 parts of chlorinated butyl rubber are added to an open mill and mixed for 5 minutes, and then 8 parts of the microcapsule nano-enhancer prepared in Example 2, 1 part of antioxidant NDPA, 1 part of antioxidant BLE, 1 part of sulfur, 0.25 parts of vulcanization accelerator monothiuram sulfide, 0.25 parts of vulcanization activator monothiuram sulfide and 5 parts of castor oil are added in sequence, and mixed evenly to obtain a vulcanized rubber material.

[0076] B2. Add the vulcanized rubber material into the mold, pressurize and mold it in a high-temperature vulcanizer at 200° C. for 4 minutes; then take out the mold, cool it to room temperature, and demold it to obtain the antibacterial composite nitrile rubber.

[0077] Example 9

[0078] This embodiment provides a method for preparing medical antibacterial nano-nitrile gloves, comprising the following steps:

[0079] B1. According to parts by weight, 80 parts of the antibacterial composite nitrile rubber prepared in Example 6 and 40 parts of chlorinated butyl rubber are added to an open mill and mixed for 5 minutes, and then 10 parts of the microcapsule nano-enhancer prepared in Example 3, 1 part of antioxidant MB, 1 part of antioxidant BLE, 1 part of sulfur, 0.25 parts of vulcanization accelerator monothiuram sulfide, 0.25 parts of vulcanization activator monothiuram sulfide and 5 parts of white ointment are added in sequence, mixed evenly, and a vulcanized rubber material is obtained.

[0080] B2. Add the vulcanized rubber material into the mold, pressurize and mold it in a high-temperature vulcanizer at 200° C. for 5 minutes; then take out the mold, cool it to room temperature, and demold it to obtain the antibacterial composite nitrile rubber.

[0081] Comparative Example 1

[0082] In the medical antibacterial nano-nitrile gloves prepared in Example 9 of the present invention, cinnamic acid modified with cyanuric chloride was not used when preparing the composite nitrile rubber, and cinnamic acid was used instead of the modified antibacterial agent.

[0083] Comparative Example 2

[0084] In the medical antibacterial nano-nitrile gloves prepared in Example 9 of the present invention, the nitrile rubber is not treated with a modified antibacterial agent.

[0085] Comparative Example 3

[0086] In the medical antibacterial nano-nitrile gloves prepared in Example 9 of the present invention, when preparing the microcapsule nano-enhancer, heavy calcium carbonate, wollastonite and dolomite were not added to the micro-nano particle composite system for spheroidization treatment, and heavy calcium carbonate, wollastonite and dolomite were directly used as core materials.

[0087] Comparative Example 4

[0088] When the medical antibacterial nano-nitrile gloves were prepared in Example 9 of the present invention, no micro-nano enhancer was added.

[0089] Performance Testing:

[0090] 1. The tensile strength and elongation at break of the medical antibacterial nano-nitrile rubber prepared in Examples 7-9 were tested according to GB / T528-2009; wherein the tensile rate was 500 mm / min.

[0091] 2. The Shore A hardness of the medical antibacterial nano-nitrile rubber prepared in Examples 7-9 was tested according to GB / T531.1-2008.

[0092] 3. Under nitrogen environment, weigh 10 g of the medical antibacterial nano-nitrile rubber prepared in Examples 7-9 and place it in a crucible. Heat it from 50° C. at a rate of 10° C. / min. Use a thermogravimetric analyzer to measure the heating temperature when the mass loss rate is 50%.

[0093] 4. The minimum inhibitory concentration (MIC) of the medical antibacterial nano-nitrile rubber prepared in Examples 7-9 against Gram-negative bacteria was tested. The specific test results are shown in the following table:

[0094] Table 1 - Performance test data table

[0095]

[0096] Data Analysis:

[0097] By analyzing the data in Table 1, the medical antibacterial nano-nitrile gloves prepared in Examples 7-9 of the present invention all have excellent mechanical properties, as shown in that the medical antibacterial nano-nitrile gloves prepared in Examples 7-9 of the present invention have excellent tensile strength, elongation at break, hardness and thermal stability values;

[0098] However, in Comparative Example 3, the inorganic material was not processed using a micro-nano particle composite system to form composite spherical particles with inner and outer layers and a dense structure, which reduced the mechanical properties of the prepared microcapsule nano-enhancer. In Comparative Example 4, no microcapsule nano-enhancer was added, which significantly reduced the mechanical properties of the prepared medical antibacterial nano-nitrile gloves.

[0099] The medical antibacterial nano-nitrile rubbers prepared in Examples 7-9 of the present invention all have excellent antibacterial properties, as shown by the fact that the medical antibacterial nano-nitrile rubbers prepared in Examples 7-9 all have relatively small minimum inhibitory concentration values ​​for Gram-negative bacteria;

[0100] However, in Comparative Example 1, cyanuric chloride-modified cinnamic acid was not used in the preparation of the composite nitrile rubber, and in Comparative Example 2, the nitrile rubber was not treated with a modified antibacterial agent, which reduced the antibacterial properties of the prepared medical antibacterial nano-nitrile gloves, as shown by an increase in the value of the minimum inhibitory concentration for Gram-negative bacteria.

[0101] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0102] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0103] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A medical antibacterial nano-nitrile glove, characterized in that: The invention comprises the following components in parts by weight: 60-80 parts of antibacterial composite nitrile rubber, 20-40 parts of chlorinated butyl rubber, 5-10 parts of microcapsule nano-enhancer, 2-3 parts of anti-aging aid, 2-5 parts of vulcanization aid and 5-10 parts of plasticizer.

2. A medical antibacterial nano-nitrile glove according to claim 1, characterized in that: The preparation method of the antibacterial composite nitrile rubber comprises the following steps: S1. Mix cinnamic acid, cyanuric chloride, sodium carbonate and ethanol evenly to obtain a premix; react the premix at 50-60°C for 2-3h, then heat to 70-75°C, and react at this temperature for 2-3h; then heat to 80-90°C, evaporate the ethanol solvent, and obtain a solid modified antibacterial agent; S2, adding the modified antibacterial agent and the nitrile rubber into a two-roll mill and uniformly dispersing them to obtain a mixture; adding the mixture into a double-roll mill plastic to obtain an antibacterial composite nitrile rubber.

3. A medical antibacterial nano-nitrile glove according to claim 2, characterized in that: In step S1, the dosage ratio of cinnamic acid, cyanuric chloride, sodium carbonate and ethanol is 50-60g:18g:5g:250mL; in step S2, the dosage ratio of modified antibacterial agent and nitrile rubber is 1-5g:50g; the plasticizing temperature is 120-150°C and the plasticizing time is 5-10min.

4. The medical antibacterial nano-nitrile gloves according to claim 3, characterized in that: The preparation method of the microcapsule nano-enhancer comprises the following steps: A1. Grinding heavy calcium carbonate to 300-500 μm to obtain mother particles; grinding wollastonite and dolomite to 30-50 μm to obtain daughter particles; adding the mother particles and daughter particles to a micro-nano particle composite system, and subjecting them to composite and spherical treatment to obtain composite spherical particles; A2, methanol and trichlorocyanuric acid silicon react at 20-30°C for 2-3h to obtain a product; the product is split and a fraction of polymethoxysilane is intercepted; A3, gelatin and deionized water are mixed, heated and stirred until completely dissolved; then casein and polymethoxysilane are added, and 1 mol / L NaOH solution is added dropwise to adjust the pH value of the mixed liquid to 8-9, so that the casein is completely dissolved to obtain a mixed solution; the mixed solution is first reacted at 80-90° C. for 2-3 hours, and then allowed to stand at room temperature for 24 hours to obtain a wall material solution; A4. Add the composite spherical particles to the wall material solution, then adjust the pH value of the wall material solution to 2-3 with 1 mol / L citric acid, and prepare a nano-scale microcapsule enhancer by spray drying.

5. The medical antibacterial nano-nitrile gloves according to claim 4, characterized in that: In step A1, the ratio of wollastonite to dolomite is 10:10, and the ratio of mother particles to daughter particles is 20:10, based on weight. The rotor speed of the PCS system is 2000-3000 r / min, and the processing time is 10-20 min.

6. The medical antibacterial nano-nitrile gloves according to claim 5, characterized in that: In step A2, the usage ratio of methanol and trichlorocyanuric acid silicon is 96g:100-135g; in step A3, the usage ratio of gelatin, deionized water, casein and polymethoxysilane is 15g:300mL:5g:10-20g; in step A4, the usage ratio of composite spherical particles and wall material solution is 50-60g:100mL.

7. A method for preparing the medical antibacterial nano-nitrile gloves as claimed in claim 6, characterized in that: The following steps are involved: B1, adding the antibacterial composite nitrile rubber and chlorinated butyl rubber into an open mill for mixing, and then sequentially adding an anti-aging agent, a vulcanizing agent and a plasticizer, and under the shearing action of a double roller, each component is in a cutting and mixing state to obtain a vulcanized rubber material; B2. Add the vulcanized rubber material into the mold, press-form it in a high-temperature vulcanizer, then take out the mold, cool it to room temperature, and demould it to obtain the antibacterial composite nitrile rubber.

8. The method for preparing a medical antibacterial nano-nitrile glove according to claim 7, characterized in that: In step B1, the amount ratio of the antibacterial composite nitrile rubber, chlorinated butyl rubber, antioxidant, vulcanization aid and plasticizer is 60-80:20-40:2-3:2-5:5-10 in parts by weight; the antioxidant includes 10 parts of naphthylamine antioxidant and 10 parts of ketoamine antioxidant in parts by weight, the naphthylamine antioxidant is any one of antioxidant A, antioxidant MB and antioxidant NDPA, and the ketoamine antioxidant includes any one of antioxidant RD and antioxidant BLE; the vulcanization aid includes 2-5 parts of sulfur, 0.5 parts of vulcanization accelerator and 0.5 parts of vulcanization activator in parts by weight, the vulcanization accelerator is thiuram monosulfide, and the vulcanization activator is zinc oxide; the plasticizer is any one of black ointment, white ointment or castor oil.

9. The method for preparing a medical antibacterial nano-nitrile glove according to claim 8, characterized in that: In step B2, the vulcanization temperature is 200° C. and the vulcanization time is 3-5 minutes.

Citation Information

Patent Citations

  • Preparation method of antibacterial and wear-proof medical rubber gloves

    CN108017812A

  • Composite rubber material and preparation method thereof

    CN110218372A

  • Antibacterial and wear-resistant medical rubber gloves and preparation process thereof

    CN115286849A

  • Oil-resistant antiskid protective glove and preparation method thereof

    CN117322695A

Cited By

  • Composite butyronitrile glove as well as preparation method and application thereof

    CN119523195A

  • A composite nitrile glove and its preparation method and application

    CN119523195B