Polyethylene rotational molding modified material resistant to photo-thermal aging and preparation method thereof

By adding modifiers and modified fillers to the polyethylene rotomolding material, and processing them during the double screw extrusion and deionized water stirring, the aging problem of polyethylene rotomolding material under high temperature and light is solved, and the problem of aging of polyethylene rotomolding material under high temperature and light is improved. The heat and light resistance of the material.

CN118931007APending Publication Date: 2024-11-12GUANGDONG RUITANG PLASTIC TECH CO LTD

Patent Information

Application Number
CN202411048608.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing polyethylene rotomolding materials tend to age under high temperature environments or after long-term lighting, resulting in degradation in performance and affecting the use effect.

Method used

Using a preparation method of anti-photothermal aging polyethylene rotomolding modified material, linear low-density polyethylene, metallocene polyethylene rotomolding material, modifier and modified filler are processed during the twin screw extrusion process. Heat and stir in deionized water, cross-linking of the modifier side chain and surface hydrolyzing grafting of the modified filler to enhance the heat and light resistance of the material.

Benefits of technology

It significantly improves the heat-resistant aging properties and photo-aging properties of the material, and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974223300000131
    Figure BDA0004974223300000131
Patent Text Reader

Abstract

The invention discloses a photo-thermal aging resistant polyethylene rotational molding modified material and a preparation method thereof, and the modified material comprises the following raw materials: linear low density polyethylene, metallocene polyethylene rotational molding material, a modifier, dicumyl peroxide and a modified filler, in the extrusion process of the linear low-density polyethylene, the metallocene polyethylene rotational plastic, the modifier and the modified filler, double bonds of a side chain of the modifier can be cross-linked with the linear low-density polyethylene and the metallocene polyethylene rotational plastic, and heating and stirring are performed in deionized water; the siloxane on the side chain of the modifier and the siloxane on the surface of the modified filler are hydrolyzed and grafted, so that the thermal aging resistance is improved, the side chain of the modifier contains a hindered amine structure and a phosphite structure, and the light aging resistance of the modified material can be improved by compounding the modifier with the modified filler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyethylene rotomolding material preparation, and in particular to a light-heat-aging resistant polyethylene rotomolding modified material and a preparation method thereof. Background Art

[0002] Rotomolding is also known as rotational molding, rotational molding, rotational molding, rotational casting, rotational molding, etc. Its working principle is: a certain amount of powdered resin is loaded into a cold mold, and after the mold is closed, the mold is driven by the rotomolding machine to slowly revolve and rotate around two mutually perpendicular rotating shafts while heating, so that the resin in the cavity is melted and evenly coated on the entire mold cavity surface with the help of gravity and centrifugal force, and finally the hollow product is obtained by cooling and demolding. Rotomolding has many characteristics: rotomolding equipment and molds are inexpensive and have a long service life; the molding of complex parts does not require post-assembly; multiple products and multiple colors can be molded at the same time; less scrap is generated. Rotomolding products are used in many fields, including children's outdoor toys, road facilities, boats, etc., fresh-keeping boxes and anti-corrosion boxes in the logistics field, garbage buried barrels and septic tanks in the environmental protection field, and vehicle decorative parts, fuel tanks, water tanks, etc. in the industrial field. However, the existing polyethylene rotomolding materials will age significantly in high temperature environments or after long-term light exposure, resulting in a decrease in their own performance, which in turn affects the use of materials. Summary of the invention

[0003] The purpose of the present invention is to provide a polyethylene rotomolding modified material resistant to light and heat aging and a preparation method thereof, so as to solve the problem that the light and heat aging resistance of polyethylene rotomolding modified materials at the current stage is generally poor.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a polyethylene rotomolding modified material resistant to light and heat aging, specifically comprising the following steps:

[0006] Linear low density polyethylene, metallocene polyethylene roto-plastic, modifier, diisopropylbenzene peroxide and modified filler are added into a twin-screw extruder, and extruded and cooled under the conditions of 80°C in zone 1, 130°C in zone 2, 180°C in zone 3, 230°C in zone 4, 230°C in zone 5 and 230°C in die head. The mixture is placed in deionized water and stirred for 1-1.5h at a speed of 60-80r / min and a temperature of 80-90°C to obtain a polyethylene roto-molding modified material resistant to light and heat aging.

[0007] Furthermore, the weight ratio of the linear low-density polyethylene, metallocene polyethylene roto-plastic, modifier and modified filler is 30-40:80-100:0.5-2:10-15, the amount of diisopropyl peroxide is 2‰ of the mass of the modifier, and the density of the linear low-density polyethylene is 0.939 g·cm-3 , melt index 5.8g·(10min) -1 The density of metallocene polyethylene plastic is 0.933 g·cm -3 , melt index 5.8g·(10min) -1 .

[0008] Further, the modifier is prepared by the following steps:

[0009] Step A1: 1,2,2,6,6-pentamethylpiperidinol, acrylic acid, dibutyltin oxide and DMF are mixed uniformly, and reacted at a speed of 120-150 r / min and a temperature of 140-150° C. for 10-15 hours to obtain intermediate 1; octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed uniformly, nitrogen is introduced for protection, and reacted at a speed of 200-300 r / min and a temperature of 90-95° C. for 3-5 hours to obtain bisaminopolysiloxane;

[0010] Step A2: bisaminopolysiloxane, KH560 and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 6-8 hours at a speed of 120-150 r / min, a temperature of 40-50° C., and a pH value of 11-12 to obtain intermediate 2. Intermediate 2, phosphorus trichloride, triethylamine and toluene are mixed evenly, and the reaction is carried out for 3-5 hours at a speed of 150-200 r / min and a temperature of 70-75° C., and then p-nitrophenol is added and the reaction is continued for 2-3 hours to obtain intermediate 3;

[0011] Step A3: The intermediate 3, tin powder, concentrated hydrochloric acid and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 1-1.5 hours at a speed of 120-150 r / min and a temperature of 90-95°C, and ammonia water is added until the pH value is 8 to obtain the intermediate 4. The intermediate 4, maleic anhydride and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 1-1.5 hours at a speed of 150-200 r / min and a temperature of 55-60°C, and triethylamine, acetic anhydride and nickel acetate are added, and the reaction is continued for 2-3 hours to obtain the modifier.

[0012] Furthermore, the molar ratio of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid described in step A1 is 1:1, the amount of dibutyltin oxide used is 1% of the total mass of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid, and the molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 1.2:1:2:3.

[0013] Furthermore, the molar ratio of the amino group on the bisaminopolysiloxane described in step A2 to KH560 is 1:2, and the molar ratio of the intermediate 2, phosphorus trichloride, triethylamine and p-nitrophenol is 1:2:2.2:2.

[0014] Furthermore, the usage ratio of the intermediate 3, tin powder and concentrated hydrochloric acid in step A3 is 5 mmol:2 g:5 mL, the mass fraction of concentrated hydrochloric acid is 36%, and the molar ratio of the intermediate 4, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 1:2.1:2.1:4.2:0.5.

[0015] Further, the modified filler is prepared by the following steps:

[0016] Step B1: Hexadecyltrimethylammonium bromide, methanol and deionized water are mixed uniformly, stirred at a speed of 120-150 r / min and a temperature of 40-50° C., and concentrated ammonia water and ethyl acetate are added, stirred for 5-10 min, ethyl orthosilicate and KH570 are added, and the reaction is carried out for 10-15 h, and the supernatant is removed by centrifugation, and the substrate is added to a hydrochloric acid solution, stirred at a speed of 150-200 r / min and a temperature of 20-25° C. for 30-40 min, and the filtrate is filtered to remove the filtrate, and the filter cake is added to an acetic acid solution, and stirred at a speed of 600-800 r / min for 30-40 min to obtain functionalized silica;

[0017] Step B2: Disperse functionalized silica in acetic acid solution, stir and add tetrabutyl titanate and deionized water at a speed of 300-500r / min and a temperature of 20-25°C, heat to 140-150°C, perform hydrothermal reaction for 10-15h, filter and wash to neutrality to obtain modified silica, mix the modified silica, 3-mercaptopropyltrimethoxysilane, benzophenone and toluene evenly, react for 1-1.5h at a speed of 150-200r / min, a temperature of 25-30°C and irradiation with 365nm ultraviolet light to obtain a modified filler.

[0018] Furthermore, the dosage ratio of hexadecyltrimethylammonium bromide, methanol, deionized water, concentrated ammonia water, ethyl acetate, tetraethyl orthosilicate and KH570 described in step B1 is 150 mg: 10 mL: 5 mL: 5 mL: 1.5 mL: 0.6 mL: 0.2 mL, the mass fraction of concentrated ammonia water is 27%, the concentration of hydrochloric acid solution is 2 mol / L, and the volume fraction of acetic acid solution is 5%.

[0019] Furthermore, the dosage ratio of the functionalized silica, acetic acid solution, tetrabutyl titanate and deionized water described in step B2 is 1g:30mL:1mL:5mL, the volume fraction of the acetic acid solution is 5%, the molar ratio of the double bond on the modified silica and 3-mercaptopropyltrimethoxysilane is 1:1, and the amount of 3-mercaptopropyltrimethoxysilane on benzophenone is 5‰ by mass.

[0020] Beneficial effects of the present invention: A light-heat-aging-resistant polyethylene rotational molding modified material comprises the following raw materials: linear low-density polyethylene, metallocene polyethylene rotational molding plastic, a modifier, dicumyl peroxide and a modified filler, the modifier is reacted with 1,2,2,6,6-pentamethylpiperidinol and acrylic acid, so that the alcohol hydroxyl group on 1,2,2,6,6-pentamethylpiperidinol reacts with the carboxyl group on acrylic acid to obtain an intermediate 1, octamethylcyclotetrasiloxane and 2,4,6,8-tetramethylcyclotetrasiloxane are ring-opened, and then reacted and polymerized with 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane to obtain a bisaminopolysiloxane. alkane, react bisaminopolysiloxane with KH560, so that the amino group on the bisaminopolysiloxane reacts with the epoxy group on KH560 to obtain intermediate 2, react intermediate 2 with phosphorus trichloride, so that the two amino groups on one side of intermediate 2 react with the chlorine atom sites on phosphorus trichloride, then add p-nitrophenol, so that the phenolic hydroxyl group on p-nitrophenol reacts with the remaining chlorine atom sites to obtain intermediate 3, reduce intermediate 3 with tin powder, so that the nitro group on intermediate 3 is converted into amino group, to obtain intermediate 4, react intermediate 4 with maleic anhydride, so that the amino group on intermediate 4 and maleic anhydride undergo a ring-opening reaction and then a ring-closing reaction to obtain a modifier.

[0021] The modified filler uses hexadecyltrimethylammonium bromide as a template, hydrolyzes and polymerizes ethyl orthosilicate and KH570, and then uses hydrochloric acid and acetic acid to remove the template to obtain functionalized silica, hydrolyzes and polymerizes tetrabutyl titanate, and embeds nano-titanium dioxide in micropores on the functionalized silica to obtain modified silica, and irradiates the modified silica and 3-mercaptopropyltrimethoxysilane with ultraviolet light so that the double bond on the modified silica reacts with the mercapto group on the 3-mercaptopropyltrimethoxysilane to obtain the modified filler.

[0022] During the extrusion process of linear low-density polyethylene, metallocene polyethylene roto-plastics, modifiers and modified fillers, the double bonds in the side chains of the modifiers can cross-link with the linear low-density polyethylene and metallocene polyethylene roto-plastics, and are heated and stirred in deionized water, so that the siloxane in the side chains of the modifiers and the siloxane on the surface of the modified fillers are hydrolyzed and grafted, thereby increasing the heat aging resistance. The side chains of the modifiers contain hindered amine structures and phosphite structures, and compounding with modified fillers can improve the light aging resistance of the modified materials. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A method for preparing a polyethylene rotomolding modified material resistant to light and heat aging, specifically comprising the following steps:

[0026] Linear low density polyethylene, metallocene polyethylene roto-plastic, modifier, diisopropylbenzene peroxide and modified filler are added into a twin-screw extruder, and extruded and cooled under the conditions of 80°C in zone 1, 130°C in zone 2, 180°C in zone 3, 230°C in zone 4, 230°C in zone 5 and 230°C in die head. Then, the extruded material is placed in deionized water and stirred for 1 hour at a speed of 60 r / min and a temperature of 80°C to obtain a polyethylene roto-molding modified material resistant to light and heat aging.

[0027] The weight ratio of the linear low-density polyethylene, metallocene polyethylene roto-plastic, modifier and modified filler is 30:80:0.5:10, the amount of diisopropyl peroxide is 2‰ of the mass of the modifier, and the density of the linear low-density polyethylene is 0.939 g·cm -3 , melt index 5.8g·(10min) -1 The density of metallocene polyethylene plastic is 0.933 g·cm -3 , melt index 5.8g·(10min) -1 .

[0028] The modifier is prepared by the following steps:

[0029] Step A1: 1,2,2,6,6-pentamethylpiperidinol, acrylic acid, dibutyltin oxide and DMF were mixed uniformly, and reacted at a speed of 120 r / min and a temperature of 140° C. for 10 hours to obtain intermediate 1; octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide were mixed uniformly, nitrogen was introduced for protection, and the reaction was carried out at a speed of 200 r / min and a temperature of 90° C. for 3 hours to obtain bisaminopolysiloxane;

[0030] Step A2: bisaminopolysiloxane, KH560 and DMF were mixed evenly, nitrogen was introduced for protection, and the reaction was carried out for 6 hours at a speed of 120 r / min, a temperature of 40° C. and a pH value of 11 to obtain intermediate 2. Intermediate 2, phosphorus trichloride, triethylamine and toluene were mixed evenly, and the reaction was carried out for 3 hours at a speed of 150 r / min and a temperature of 70° C., and then p-nitrophenol was added and the reaction was continued for 2 hours to obtain intermediate 3;

[0031] Step A3: The intermediate 3, tin powder, concentrated hydrochloric acid and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out at a speed of 120 r / min and a temperature of 90°C for 1 hour. Ammonia water is added until the pH value is 8 to obtain the intermediate 4. The intermediate 4, maleic anhydride and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out at a speed of 150 r / min and a temperature of 55°C for 1 hour. After that, triethylamine, acetic anhydride and nickel acetate are added, and the reaction is continued for 2 hours to obtain the modifier.

[0032] The molar ratio of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid described in step A1 is 1:1, the amount of dibutyltin oxide used is 1% of the mass sum of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid, and the molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 1.2:1:2:3.

[0033] The molar ratio of the amino group on the bisaminopolysiloxane described in step A2 to KH560 is 1:2, and the molar ratio of intermediate 2, phosphorus trichloride, triethylamine and p-nitrophenol is 1:2:2.2:2.

[0034] The usage ratio of intermediate 3, tin powder and concentrated hydrochloric acid in step A3 is 5 mmol:2 g:5 mL, the mass fraction of concentrated hydrochloric acid is 36%, and the molar ratio of intermediate 4, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 1:2.1:2.1:4.2:0.5.

[0035] The modified filler is prepared by the following steps:

[0036] Step B1: Hexadecyltrimethylammonium bromide, methanol and deionized water are mixed uniformly, stirred at a speed of 120 r / min and a temperature of 40°C, and concentrated ammonia water and ethyl acetate are added, stirred for 5 minutes, and tetraethyl orthosilicate and KH570 are added. After reacting for 10 hours, the supernatant is removed by centrifugation, and the substrate is added to a hydrochloric acid solution, stirred for 30 minutes at a speed of 150 r / min and a temperature of 20°C, and the filtrate is filtered to remove the filtrate, and the filter cake is added to an acetic acid solution, stirred for 30 minutes at a speed of 600 r / min to obtain functionalized silica;

[0037] Step B2: Disperse functionalized silica in acetic acid solution, stir and add tetrabutyl titanate and deionized water at a speed of 300 r / min and a temperature of 20°C, heat to 140°C, hydrothermally react for 10 hours, filter and wash to neutrality to obtain modified silica, mix the modified silica, 3-mercaptopropyltrimethoxysilane, benzophenone and toluene evenly, react at a speed of 150 r / min, a temperature of 25°C and irradiation with 365nm ultraviolet light for 1 hour to obtain a modified filler.

[0038] The dosage ratio of hexadecyltrimethylammonium bromide, methanol, deionized water, concentrated ammonia water, ethyl acetate, tetraethyl orthosilicate and KH570 described in step B1 is 150 mg: 10 mL: 5 mL: 5 mL: 1.5 mL: 0.6 mL: 0.2 mL, the mass fraction of concentrated ammonia water is 27%, the concentration of hydrochloric acid solution is 2 mol / L, and the volume fraction of acetic acid solution is 5%.

[0039] The dosage ratio of the functionalized silica, acetic acid solution, tetrabutyl titanate and deionized water described in step B2 is 1g:30mL:1mL:5mL, the volume fraction of the acetic acid solution is 5%, the molar ratio of the double bond on the modified silica and 3-mercaptopropyltrimethoxysilane is 1:1, and the amount of 3-mercaptopropyltrimethoxysilane on benzophenone is 5‰ by mass.

[0040] Example 2

[0041] A method for preparing a light-heat-aging-resistant polyethylene rotational molding modified material specifically comprises the following steps:

[0042] Linear low density polyethylene, metallocene polyethylene roto-plastic, modifier, diisopropylbenzene peroxide and modified filler are added into a twin-screw extruder, and extruded and cooled under the conditions of 80°C in zone 1, 130°C in zone 2, 180°C in zone 3, 230°C in zone 4, 230°C in zone 5 and 230°C in die head. Then, the extruded material is placed in deionized water and stirred for 1.5 hours at a speed of 60 r / min and a temperature of 85°C to obtain a polyethylene roto-molding modified material resistant to light and heat aging.

[0043] The weight ratio of the linear low-density polyethylene, metallocene polyethylene roto-plastic, modifier and modified filler is 35:90:1.2:13, the amount of diisopropyl peroxide is 2‰ of the mass of the modifier, and the density of the linear low-density polyethylene is 0.939 g·cm -3 , melt index 5.8g·(10min) -1 The density of metallocene polyethylene plastic is 0.933 g·cm -3 , melt index 5.8g·(10min) -1 .

[0044] The modifier is prepared by the following steps:

[0045] Step A1: 1,2,2,6,6-pentamethylpiperidinol, acrylic acid, dibutyltin oxide and DMF were mixed uniformly, and reacted at a speed of 120 r / min and a temperature of 145° C. for 13 hours to obtain intermediate 1; octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide were mixed uniformly, nitrogen was introduced for protection, and reacted at a speed of 200 r / min and a temperature of 95° C. for 4 hours to obtain bisaminopolysiloxane;

[0046] Step A2: bisaminopolysiloxane, KH560 and DMF were mixed evenly, nitrogen was introduced for protection, and the reaction was carried out for 7 hours at a speed of 120 r / min, a temperature of 45° C. and a pH value of 12 to obtain intermediate 2. Intermediate 2, phosphorus trichloride, triethylamine and toluene were mixed evenly, and the reaction was carried out for 4 hours at a speed of 150 r / min and a temperature of 75° C., and then p-nitrophenol was added and the reaction was continued for 2.5 hours to obtain intermediate 3;

[0047] Step A3: The intermediate 3, tin powder, concentrated hydrochloric acid and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out at a speed of 120 r / min and a temperature of 95°C for 1 hour. Ammonia water is added until the pH value is 8 to obtain the intermediate 4. The intermediate 4, maleic anhydride and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out at a speed of 150 r / min and a temperature of 58°C for 1.5 hours. Triethylamine, acetic anhydride and nickel acetate are added, and the reaction is continued for 3 hours to obtain the modifier.

[0048] The molar ratio of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid described in step A1 is 1:1, the amount of dibutyltin oxide used is 1% of the mass sum of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid, and the molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 1.2:1:2:3.

[0049] The molar ratio of the amino group on the bisaminopolysiloxane described in step A2 to KH560 is 1:2, and the molar ratio of intermediate 2, phosphorus trichloride, triethylamine and p-nitrophenol is 1:2:2.2:2.

[0050] The usage ratio of intermediate 3, tin powder and concentrated hydrochloric acid in step A3 is 5 mmol:2 g:5 mL, the mass fraction of concentrated hydrochloric acid is 36%, and the molar ratio of intermediate 4, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 1:2.1:2.1:4.2:0.5.

[0051] The modified filler is prepared by the following steps:

[0052] Step B1: Hexadecyltrimethylammonium bromide, methanol and deionized water are mixed uniformly, stirred at a speed of 120 r / min and a temperature of 45°C, and concentrated ammonia water and ethyl acetate are added, stirred for 8 minutes, and tetraethyl orthosilicate and KH570 are added. After reacting for 13 hours, the supernatant is removed by centrifugation, and the substrate is added to a hydrochloric acid solution, stirred for 35 minutes at a speed of 150 r / min and a temperature of 25°C, and the filtrate is filtered to remove the filtrate, and the filter cake is added to an acetic acid solution, stirred for 35 minutes at a speed of 600 r / min, to obtain functionalized silica;

[0053] Step B2: Disperse functionalized silica in acetic acid solution, stir and add tetrabutyl titanate and deionized water at a speed of 300 r / min and a temperature of 25°C, heat to 145°C, hydrothermally react for 13 hours, filter and wash to neutrality to obtain modified silica, mix the modified silica, 3-mercaptopropyltrimethoxysilane, benzophenone and toluene evenly, react at a speed of 200 r / min, a temperature of 28°C and irradiation with 365nm ultraviolet light for 1.5 hours to obtain a modified filler.

[0054] The dosage ratio of hexadecyltrimethylammonium bromide, methanol, deionized water, concentrated ammonia water, ethyl acetate, tetraethyl orthosilicate and KH570 described in step B1 is 150 mg: 10 mL: 5 mL: 5 mL: 1.5 mL: 0.6 mL: 0.2 mL, the mass fraction of concentrated ammonia water is 27%, the concentration of hydrochloric acid solution is 2 mol / L, and the volume fraction of acetic acid solution is 5%.

[0055] The dosage ratio of the functionalized silica, acetic acid solution, tetrabutyl titanate and deionized water described in step B2 is 1g:30mL:1mL:5mL, the volume fraction of the acetic acid solution is 5%, the molar ratio of the double bond on the modified silica and 3-mercaptopropyltrimethoxysilane is 1:1, and the amount of 3-mercaptopropyltrimethoxysilane on benzophenone is 5‰ by mass.

[0056] Example 3

[0057] A method for preparing a light-heat-aging-resistant polyethylene rotational molding modified material specifically comprises the following steps:

[0058] Linear low density polyethylene, metallocene polyethylene roto-plastic, modifier, diisopropylbenzene peroxide and modified filler are added into a twin-screw extruder, and extruded and cooled under the conditions of zone 1 temperature of 80°C, zone 2 temperature of 130°C, zone 3 temperature of 180°C, zone 4 temperature of 230°C, zone 5 temperature of 230°C and head temperature of 230°C. Then, the mixture is placed in deionized water and stirred for 1.5 hours at a speed of 80 r / min and a temperature of 90°C to obtain a polyethylene roto-molding modified material resistant to light and heat aging.

[0059] The weight ratio of the linear low-density polyethylene, metallocene polyethylene rotoplastic, modifier and modified filler is 40:100:2:15, the amount of diisopropyl peroxide is 2‰ of the mass of the modifier, and the density of the linear low-density polyethylene is 0.939 g·cm -3 , melt index 5.8g·(10min) -1 The density of metallocene polyethylene plastic is 0.933 g·cm -3 , melt index 5.8g·(10min) -1 .

[0060] The modifier is prepared by the following steps:

[0061] Step A1: 1,2,2,6,6-pentamethylpiperidinol, acrylic acid, dibutyltin oxide and DMF were mixed uniformly, and reacted at a speed of 150 r / min and a temperature of 150° C. for 15 hours to obtain intermediate 1; octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide were mixed uniformly, nitrogen was introduced for protection, and the reaction was carried out at a speed of 300 r / min and a temperature of 95° C. for 5 hours to obtain bisaminopolysiloxane;

[0062] Step A2: bisaminopolysiloxane, KH560 and DMF were mixed evenly, nitrogen was introduced for protection, and the reaction was carried out for 8 hours at a speed of 150 r / min, a temperature of 50° C. and a pH value of 12 to obtain intermediate 2. Intermediate 2, phosphorus trichloride, triethylamine and toluene were mixed evenly, and the reaction was carried out for 5 hours at a speed of 200 r / min and a temperature of 75° C., and then p-nitrophenol was added and the reaction was continued for 3 hours to obtain intermediate 3;

[0063] Step A3: The intermediate 3, tin powder, concentrated hydrochloric acid and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 1.5 hours at a speed of 150 r / min and a temperature of 95°C. Ammonia water is added until the pH value is 8 to obtain the intermediate 4. The intermediate 4, maleic anhydride and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 1.5 hours at a speed of 200 r / min and a temperature of 60°C. Triethylamine, acetic anhydride and nickel acetate are added, and the reaction is continued for 3 hours to obtain the modifier.

[0064] The molar ratio of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid described in step A1 is 1:1, the amount of dibutyltin oxide used is 1% of the mass sum of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid, and the molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 1.2:1:2:3.

[0065] The molar ratio of the amino group on the bisaminopolysiloxane described in step A2 to KH560 is 1:2, and the molar ratio of intermediate 2, phosphorus trichloride, triethylamine and p-nitrophenol is 1:2:2.2:2.

[0066] The usage ratio of intermediate 3, tin powder and concentrated hydrochloric acid in step A3 is 5 mmol:2 g:5 mL, the mass fraction of concentrated hydrochloric acid is 36%, and the molar ratio of intermediate 4, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 1:2.1:2.1:4.2:0.5.

[0067] The modified filler is prepared by the following steps:

[0068] Step B1: Hexadecyltrimethylammonium bromide, methanol and deionized water are mixed uniformly, stirred at a speed of 150 r / min and a temperature of 50°C, and concentrated ammonia water and ethyl acetate are added, stirred for 10 min, ethyl orthosilicate and KH570 are added, reacted for 15 h, centrifuged to remove the supernatant, the substrate is added to a hydrochloric acid solution, stirred at a speed of 200 r / min and a temperature of 25°C for 40 min, the filtrate is filtered out, the filter cake is added to an acetic acid solution, stirred at a speed of 800 r / min for 40 min, and functionalized silica is obtained;

[0069] Step B2: Disperse functionalized silica in acetic acid solution, stir and add tetrabutyl titanate and deionized water at a speed of 500 r / min and a temperature of 25°C, heat to 150°C, hydrothermally react for 15 hours, filter and wash to neutrality to obtain modified silica, mix the modified silica, 3-mercaptopropyltrimethoxysilane, benzophenone and toluene evenly, react at a speed of 200 r / min, a temperature of 30°C and irradiation with 365nm ultraviolet light for 1.5 hours to obtain a modified filler.

[0070] The dosage ratio of hexadecyltrimethylammonium bromide, methanol, deionized water, concentrated ammonia water, ethyl acetate, tetraethyl orthosilicate and KH570 described in step B1 is 150 mg: 10 mL: 5 mL: 5 mL: 1.5 mL: 0.6 mL: 0.2 mL, the mass fraction of concentrated ammonia water is 27%, the concentration of hydrochloric acid solution is 2 mol / L, and the volume fraction of acetic acid solution is 5%.

[0071] The dosage ratio of the functionalized silica, acetic acid solution, tetrabutyl titanate and deionized water described in step B2 is 1g:30mL:1mL:5mL, the volume fraction of the acetic acid solution is 5%, the molar ratio of the double bond on the modified silica and 3-mercaptopropyltrimethoxysilane is 1:1, and the amount of 3-mercaptopropyltrimethoxysilane on benzophenone is 5‰ by mass.

[0072] Comparative Example 1

[0073] Compared with Example 1, this comparative example uses Intermediate 1 to replace the modifier, and the remaining steps are the same.

[0074] Comparative Example 2

[0075] Compared with Example 1, this comparative example uses ethylene oxide instead of KH560, and the other steps are the same.

[0076] Comparative Example 3

[0077] Compared with Example 1, this comparative example uses bisaminopolysiloxane to replace intermediate 4, and the remaining steps are the same.

[0078] Comparative Example 4

[0079] Compared with Example 1, this comparative example uses nano silicon dioxide instead of the modified filler, and the other steps are the same.

[0080] Comparative Example 5

[0081] Compared with Example 1, this comparative example uses nano titanium dioxide to replace the modified filler, and the other steps are the same.

[0082] The modified materials obtained in Examples 1-3 and Comparative Examples 1-5 were made into Type I specimens according to the standard of GB / T10402-2006, and the tensile strength was tested at a tensile speed of 50 mm / min. The tensile strength after heat aging was tested at a temperature of 135°C for 168 h. The tensile strength after heat aging was tested at an irradiation intensity of 600 W / m 2 The cumulative irradiation is 400kWh / m 2 , detect the tensile strength after light aging, calculate the tensile strength retention rate after light and heat aging, and the test results are shown in the following table.

[0083]

[0084] It can be seen from the above table that the present invention has a good light and heat aging resistance effect.

[0085] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a light-heat-aging-resistant polyethylene rotational molding modified material, characterized in that: The specific steps include: Linear low density polyethylene, metallocene polyethylene roto-plastic, modifier, diisopropylbenzene peroxide and modified filler are added into a twin-screw extruder, and extruded and cooled under the conditions of 80°C in zone 1, 130°C in zone 2, 180°C in zone 3, 230°C in zone 4, 230°C in zone 5 and 230°C in die head. The mixture is placed in deionized water and stirred for 1-1.5h at a speed of 60-80r / min and a temperature of 80-90°C to obtain a polyethylene roto-molding modified material resistant to light and heat aging.

2. The method for preparing a light-heat-aging-resistant polyethylene rotational molding modified material according to claim 1, characterized in that: The weight ratio of the linear low-density polyethylene, the metallocene polyethylene rotoplastic, the modifier and the modified filler is 30-40:80-100:0.5-2:10-15.

3. The method for preparing a light-heat-aging resistant polyethylene rotational molding modified material according to claim 1, characterized in that: The modifier is prepared by the following steps: Step A1: 1,2,2,6,6-pentamethylpiperidinol, acrylic acid, dibutyltin oxide and DMF are mixed and reacted to obtain intermediate 1, octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed uniformly, and nitrogen is introduced for protection to react to obtain bisaminopolysiloxane; Step A2: bisaminopolysiloxane, KH560 and DMF are mixed evenly, and nitrogen is introduced to react to obtain intermediate 2. Intermediate 2, phosphorus trichloride, triethylamine and toluene are mixed to react, and then p-nitrophenol is added to continue the reaction to obtain intermediate 3; Step A3: The intermediate 3, tin powder, concentrated hydrochloric acid and DMF are mixed evenly, nitrogen is introduced for protection, and ammonia water is added until the pH value is 8 to obtain the intermediate 4. The intermediate 4, maleic anhydride and DMF are mixed evenly, nitrogen is introduced for protection, and a reaction is carried out. After that, triethylamine, acetic anhydride and nickel acetate are added, and the reaction is continued to obtain the modifier.

4. The method for preparing a light-heat-aging resistant polyethylene rotational molding modified material according to claim 3, characterized in that: The molar ratio of 1,2,2,6,6-pentamethylpiperidinol and acrylic acid in step A1 is 1:1, and the molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 1.2:1:2:

3.

5. The method for preparing a light-heat-aging resistant polyethylene rotational molding modified material according to claim 3, characterized in that: The molar ratio of the amino group on the bisaminopolysiloxane described in step A2 to KH560 is 1:2, and the molar ratio of the intermediate 2, phosphorus trichloride, triethylamine and p-nitrophenol is 1:2:2.2:

2.

6. The method for preparing a light-heat-aging resistant polyethylene rotational molding modified material according to claim 3, characterized in that: The amount ratio of intermediate 3, tin powder and concentrated hydrochloric acid in step A3 is 5mmo l:2g:5mL, and the molar ratio of intermediate 4, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 1:2.1:2.1:4.2:0.

5.

7. The method for preparing a light-heat-aging resistant polyethylene rotational molding modified material according to claim 1, characterized in that: The modified filler is prepared by the following steps: Step B1: Hexadecyltrimethylammonium bromide, methanol and deionized water are mixed and stirred, and concentrated ammonia water and ethyl acetate are added, stirred, and tetraethyl orthosilicate and KH570 are added. After reaction, the supernatant is removed by centrifugation, and the substrate is added to a hydrochloric acid solution, stirred, and the filtrate is filtered out. The filter cake is added to an acetic acid solution, stirred, and functionalized silica is obtained; Step B2: Disperse functionalized silica in acetic acid solution, stir and add tetrabutyl titanate and deionized water, heat up for hydrothermal reaction, filter and wash to neutrality to obtain modified silica, mix the modified silica, 3-mercaptopropyltrimethoxysilane, benzophenone and toluene evenly, react under ultraviolet light to obtain a modified filler.

8. The method for preparing a light-heat-aging resistant polyethylene rotational molding modified material according to claim 7, characterized in that: The usage ratio of hexadecyltrimethylammonium bromide, methanol, deionized water, concentrated aqueous ammonia, ethyl acetate, ethyl orthosilicate and KH570 described in step B1 is 150 mg: 10 mL: 5 mL: 5 mL: 1.5 mL: 0.6 mL: 0.2 mL.

9. The method for preparing a light-heat-aging resistant polyethylene rotational molding modified material according to claim 7, characterized in that: The amount ratio of the functionalized silica, acetic acid solution, tetrabutyl titanate and deionized water described in step B2 is 1 g:30 mL:1 mL:5 mL, and the molar ratio of the double bonds on the modified silica and 3-mercaptopropyltrimethoxysilane is 1:

1.

10. A light-heat-aging resistant polyethylene rotomolding modified material, characterized in that: Prepared according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Anti-scouring magnetic product coating and preparation method thereof

    CN116285552A

  • Aluminum-free composite material for pesticide packaging and preparation method thereof

    CN116535760A

  • Anti-aging polypropylene material and preparation method thereof

    CN117757187A

  • Functional reinforcing fillers modified with alkenylalkoxysilane and preparing method of the same

    US20120277361A1

Cited By

  • Anti-aging recycled PP composite material and preparation method thereof

    CN120518952A

  • Aging-resistant recycled pp composite material and preparation method thereof

    CN120518952B