Raw material preparation method of special silica gel plate with high tear resistance and low pressure change for solar laminating machine
Through the calendering, composite and vulcanization processes of silicone rubber and fabrics, high tear-resistant and low-pressure change silicone boards are prepared, which solves the problems of easy damage and volatile odors in high-temperature vacuum conditions, and achieves high performance and long life silicone plate products.
Patent Information
- Application Number
- CN202410995168.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The existing silicone plates of solar laminates are prone to damage under high temperature and vacuum conditions, and the peroxide vulcanization method has problems of volatile odor and high energy consumption, which affects its service life and quality.
Silicone rubber and fabrics are used as raw materials to prepare high tear-resistant and low-pressure change silicone boards through calendering, composite and vulcanization processes, and use modified white carbon black, polyvinyl silicone oil, hydrogen-containing silicone oil, heat-resistant agent and platinum vulcanizing agent. , surface treatment and vulcanization are carried out to form high-reinforcement and low-thickening silicone board.
It improves the tear resistance and heat aging resistance of silicone boards, reduces the compression permanent deformation rate, maintains good performance at high temperatures, and has no odor. The number of times it uses reaches more than 18,000 times, meeting the requirements of large-scale photovoltaic lamination equipment.
Smart Images

Figure BDA0004959951490000021 
Figure FDA0004959951480000011
Abstract
Description
Technical Field
[0001] The invention relates to the field of special silicone plates for solar photovoltaic component laminators, and in particular to a method for preparing raw materials of a special silicone plate for solar laminators with high tear resistance and low pressure deformation. Background Art
[0002] The working principle of the photovoltaic laminator is to press the stacked glass, EVA, connected single cells, EVA, and TPT into solar cell modules through vacuum hot pressing.
[0003] The silicone plate of the Taiyang photovoltaic module laminating machine is one of the important key accessories of the Taiyang photovoltaic module laminating machine and is an important factor in converting raw materials into photovoltaic panels.
[0004] According to the statistics of customers on the use of silicone sheets for laminators, the most obvious indentations are found in the positions around the contact components and the positions around the installed steel plates after use, and the final damage and cracking are also in these parts. The working temperature of the silicone sheet during use is 135-150℃, and the vacuum is minus 0.1 atmosphere. During use, it will go through the steps of repeated vacuuming and laminating components. The working nature of the laminator requires that the silicone sheet must have good high temperature aging resistance and low compression deformation. And the vulcanization method of the silicone sheets currently sold on the market is mostly peroxide vulcanization. Peroxide vulcanizers will be accompanied by volatile odors under high temperature conditions during use, and secondary vulcanization is required during the production process. Secondary vulcanization will increase energy consumption in the production process, and secondary vulcanization cannot completely remove volatile products. There will still be a small amount of odor generated by volatile products during subsequent customer use. According to the current customer demand for cost reduction and efficiency improvement, improving the quality and service life of silicone sheets is an active research topic in this field. Summary of the invention
[0005] The purpose of the present invention is to improve the service performance and life of the existing silica gel plate, and to provide a silica gel plate raw material with high tear resistance and low pressure deformation and a preparation method thereof.
[0006] To achieve the above object, the present invention provides a method for preparing a raw material of a silicone plate for a solar laminator with high tear resistance and low pressure deformation, wherein the raw materials of the silicone plate include: silicone rubber and fabric;
[0007] The silicone rubber and fabric are formed into a silicone plate through calendering, compounding and vulcanization;
[0008] The silicone rubber components include:
[0009] Methyl vinyl silicone rubber, modified white carbon black, polyvinyl silicone oil, hydrogen silicone oil, zinc stearate, heat resistant agent, masterbatch, vulcanizing agent.
[0010] Furthermore, the raw materials constituting the silicone rubber are recorded in parts by mass as follows:
[0011]
[0012] Furthermore, the vinyl content of the methyl vinyl silicone rubber raw rubber is between 0.03% and 8.0%, the average molecular weight of the raw rubber is between 590,000 and 700,000, and it is a compound of several raw rubbers with different vinyl contents;
[0013] The modified white carbon black has a specific surface area of 200 m 2 / g of fumed silica or precipitated silica is produced independently through the continuous silica pretreatment technology solution;
[0014] The hydrogen-containing silicone oil is a high-hydrogen-containing telomerized side hydrogen silicone oil;
[0015] The heat-resistant agent can be one or a combination of cerium oxide, cerium carbonate, iron oxide, titanium dioxide, and organosilicon ferrocene;
[0016] The ratio of the vulcanizing agent to the inhibitor is about 1:4-1:5.
[0017] A method for preparing silicone rubber comprises the following steps:
[0018] Step 1: Add the modifier and the white carbon black to be treated into the modifier continuously at a certain rate to achieve continuous treatment of the surface of the white carbon black, and prepare the required modified white carbon black in advance;
[0019] Step 2: After kneading the raw rubber with different vinyl contents and zinc stearate in a kneader for several minutes, the modified silica and polyvinyl silicone oil are added to the kneading vacuum machine in batches, and the mixture is fully stirred after each addition. After the rubber in the kneader forms a large mass each time, the modified silica can be added next time;
[0020] Step 3: After all materials are added and the rubber material is kneaded and formed, the temperature is raised for heat treatment, and then vacuumized and cooled to produce the rubber. The rubber material obtained at this time is used as the base rubber;
[0021] Step 4: Put the base rubber into the kneader, add the heat-resistant agent, hydrogen-containing silicone oil, masterbatch and vulcanizing agent, and stir well to obtain the raw material silicone rubber for the silicone plate.
[0022] Further, the white carbon black and polyvinyl silicone oil in step 2 are added in 4 portions;
[0023] The heat treatment temperature in step 2 is 160-180°C and the heat treatment time is 90-120min;
[0024] The vacuuming time in step 2 is 40-60 minutes.
[0025] A method for preparing a fabric comprises the following steps:
[0026] Step 1: After the polybutylene terephthalate fiber mesh cloth is rolled into a roll shape by a winder, it is immersed in the immersion liquid of the static sedimentation tank;
[0027] Step 2: Take out the soaked mesh and squeeze out the excess soaking liquid in the embossing roller;
[0028] Step 3: Put the mesh into the drying room for drying to obtain the desired fabric.
[0029] Furthermore, the soaking liquid temperature in S1 is set to 30-40° C., and the soaking time is 20-30 min;
[0030] The temperature of the drying chamber in S3 is set to 110-130° C., and the drying time is 40-60 min.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. By preparing modified silica in advance, the surface treatment of silica can be achieved in advance, and modified silica with high reinforcement, low thickening effect and easy dispersion can be prepared, making the subsequent mixing process more efficient and stable;
[0033] The modified silica treatment technology is based on the silanol groups on the surface of silica and the molecular structure characteristics of the silicone rubber to be reinforced. Siloxanes and silazanes of different structures are used as raw materials. Under the action of an initiator, an active modifier with a low molecular weight and a fast-reacting molecular structure (such as hydrogen-containing, hydroxyl-containing silicon nitrogen and silicon oxygen structure) is prepared. The modifier and the silica to be treated are continuously added to the modifier at different rates to achieve continuous treatment of the silica surface. The modified silica treated with this formula has high mechanical strength and high damping properties. The modified silica can be directly mixed and added to silicone rubber. The modified silica used in this formula can not only achieve a good reinforcement effect, but also improve the damping performance of silicone rubber and improve the compression deformation performance of the product.
[0034] 2. Improve the tear resistance and heat aging resistance of silicone rubber through the design and optimization of silicone rubber raw material formula to achieve high performance and high usage of silicone plates. Selecting several raw rubbers with different vinyl contents and using them in a certain proportion can improve the tear performance of silicone rubber. At the same time, the vinyl content optimized by this formula can increase the crosslinking degree of the product and reduce the compression permanent deformation rate of the product; the vinyl content in polyvinyl silicone oil is relatively concentrated, and the crosslinking density is also relatively concentrated, which can produce plastic micro-regions with relatively high strength, improve the crosslinking degree of the silicone rubber system, and greatly improve the tear strength of the product. At the same time, improve the compression permanent deformation performance; the cerium oxide, cerium carbonate, iron oxide, titanium dioxide, and organosilicon ferrocene in the heat-resistant agent are compounded in a certain proportion and added to silicone rubber. After aging at 250°C, the tensile strength of the product is still highly retained, and the heat resistance is excellent; hydrogen-containing silicone oil is used as a crosslinking agent for platinum-vulcanized silicone rubber. In addition, the molecules of hydrogen-containing silicone oil contain active hydrogen that plays a reducing role, which can effectively prevent the impurities in the rubber from oxidizing and yellowing; zinc stearate is used as a release agent; the vulcanizing agent uses a platinum vulcanization system, which can be made into a two-component AB glue and then used in combination, or it can be made into a single component and used directly; the vulcanization reaction of platinum-vulcanized silicone rubber does not produce by-products, the product recovery rate during the vulcanization process is extremely small, and there is no odor during production and use, realizing the one-time vulcanization molding of silicone plate products.
[0035] 3. The polybutylene terephthalate fiber mesh itself has excellent anti-aging, chemical reaction resistance and heat resistance. Adding the mesh impregnation process can better fix the warp and weft of the mesh, and prevent the mesh from shifting or deforming due to the extrusion of the rubber during the production of the silicone plate. At the same time, the mesh after impregnation will be more firmly combined with the silicone rubber.
[0036] 4. According to the silicone rubber and fabric provided by the present invention, the silicone plate products produced according to the three-rubber and two-cloth production process of silicone plate independently designed by Tianchen New Materials have high tear strength and low compression permanent deformation, excellent heat aging resistance, acid and alkali resistance, and the lamination times can reach more than 18,000 times, which can meet the use requirements of large-scale photovoltaic lamination equipment.
[0037] In order to better understand and implement the present invention, the present invention is described in detail below in conjunction with embodiments. DETAILED DESCRIPTION
[0038] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific implementation methods of the present invention are now described with reference to examples, but the protection scope of the present invention is not limited to the following.
[0039] Example 1
[0040] After kneading 100 parts of raw rubber with different vinyl contents and 0.17 parts of zinc stearate in a vacuum kneader for a few minutes, 36 parts of modified white carbon black and 0.7 parts of polyvinyl silicone oil were added to the vacuum kneader in 4 times. The mixture was fully stirred after each addition. After the mixed rubber sheet was uniformly formed, the temperature was raised to 160°C and hot-refined for 120 minutes. Then, vacuum-0.07MPa was evacuated, and the rubber was discharged after 40 minutes of vacuumization. The rubber obtained at this time was used as the base rubber. The base rubber was put into the kneader, and 1.5 parts of cerium oxide, 1 part of titanium dioxide, 0.5 parts of hydrogen-containing silicone oil, 1.5 parts of masterbatch and 0.2 parts of vulcanizer were added. After fully stirring, the rubber was filtered out to obtain the raw material silicone rubber for the silica gel sheet.
[0041] The polybutylene terephthalate fiber mesh cloth was immersed in the immersion liquid at 30°C for 30 minutes, and then the excess immersion liquid was squeezed out on the embossing roller, and then dried in a drying room at 110°C for 60 minutes to obtain the silicone rubber raw material for the silica gel plate.
[0042] According to the three-rubber and two-fabric process designed by our company, the silicone rubber and fabric of Example 1 are calendered, laminated and vulcanized to produce a silicone plate. The mechanical properties of the plate are tested, and the tensile strength is 13MPa, the tear strength is 45KN / M, and the compression deformation rate is 22%.
[0043] Example 2
[0044] After kneading 100 parts of raw rubber with different vinyl content and 0.2 parts of zinc stearate in a vacuum kneader for a few minutes, 55 parts of modified white carbon black and 1.3 parts of polyvinyl silicone oil were added to the vacuum kneader in 4 times. The mixture was fully stirred after each addition. After the mixed rubber sheet was evenly formed, the temperature was raised to 170°C and hot-refined for 90 minutes. Then vacuumed to -0.07MPa, and the rubber was discharged after vacuuming for 60 minutes. The rubber obtained at this time was used as the base rubber. The base rubber was put into the kneader, and 1 part of cerium oxide, 1 part of iron oxide, 1 part of organosilicon ferrocene, 0.7 parts of hydrogenated silicone oil, 1.5 parts of masterbatch and 0.3 parts of vulcanizer were added. After fully stirring, the rubber was filtered out to obtain the raw material silicone rubber for the silica gel sheet.
[0045] The polybutylene terephthalate fiber mesh cloth was immersed in the immersion liquid at 40°C for 20 minutes, the excess immersion liquid was squeezed out on the embossing roller, and the cloth was dried in a drying room at 130°C for 40 minutes to obtain the silicone rubber raw material for the silica gel plate.
[0046] According to the three-rubber and two-fabric process designed by our company, the silicone rubber and fabric of Example 1 are calendered, laminated and vulcanized to produce a silicone plate. The mechanical properties of the plate are tested, and the tensile strength is 15MPa, the tear strength is 60KN / M, and the compression deformation rate is 20%.
[0047] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention still fall within the scope covered by the present invention.
Claims
1. A method for preparing raw materials for a special silicone plate for a solar laminator with high tear resistance and low pressure change, characterized in that: The silicone plate is made of silicone rubber and fabric. The silicone rubber and fabric are formed into a silicone plate through calendering, compounding and vulcanization; The silicone rubber components include: methyl vinyl silicone rubber raw rubber, modified white carbon black, polyvinyl silicone oil, hydrogen-containing silicone oil, zinc stearate, heat-resistant agent, masterbatch and vulcanizing agent.
2. The method for preparing raw materials of a high tear resistance and low pressure deformation silicone plate for solar laminators according to claim 1, characterized in that: The raw materials that make up silicone rubber are expressed in parts by mass as follows:
3. The method for preparing raw materials of a silicone plate for solar laminator with high tear resistance and low pressure change according to claim 1, characterized in that: The vinyl content of the methyl vinyl silicone rubber raw rubber is between 0.03% and 8.0%, the average molecular weight of the raw rubber is between 590,000 and 700,000, and the raw rubber is compounded with several raw rubbers with different vinyl contents.
4. The method for preparing raw materials of a high tear resistance and low pressure deformation special silicone plate for solar laminators according to claim 2, characterized in that: The content of each component in the modified white carbon black is recorded in parts by mass as follows: 100 parts of white carbon black Modifier A1-10 parts Modifier B1-25 parts The modifier is an active modifier with low molecular weight and containing a rapidly reactive molecular structure (such as hydrogen-containing, hydroxyl-containing silicon nitrogen and silicon oxygen structure) prepared from siloxane and silazane of different structures as raw materials under the action of an initiator.
5. The method for preparing raw materials of a high tear resistance and low pressure deformation special silicone plate for solar laminator according to claim 2, characterized in that: The heat-resistant agent can be one or a combination of cerium oxide, cerium carbonate, iron oxide, titanium dioxide, and organosilicon ferrocene.
6. The method for preparing raw materials of a high tear resistance and low pressure deformation silicone plate for solar laminator according to claim 2, characterized in that: The ratio of the vulcanizing agent to the inhibitor is about 1:4-1:
5.
7. A method for preparing silicone rubber according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1: Add the modifier and the white carbon black to be treated into the modifier continuously at a certain rate to achieve continuous treatment of the surface of the white carbon black, and prepare the required modified white carbon black in advance; Step 2: After kneading the raw rubber with different vinyl contents and zinc stearate in a kneader for several minutes, the modified silica and polyvinyl silicone oil are added to the kneading vacuum machine in batches, and the mixture is fully stirred after each addition. After the rubber in the kneader forms a large mass each time, the modified silica can be added next time; Step 3: After all materials are added and the rubber material is kneaded and formed, the temperature is raised for heat treatment, and then vacuumized and cooled to produce the rubber. The rubber material obtained at this time is used as the base rubber; Step 4: Put the base rubber into the kneader, add the heat-resistant agent, hydrogen-containing silicone oil, masterbatch and vulcanizing agent, and stir well to obtain the raw material silicone rubber for the silicone plate.
8. The method for preparing silicone rubber according to claim 7, characterized in that: The modified silica and polyvinyl silicone oil in step 2 are added in 4 portions; The heat treatment temperature in step 3 is 160-180°C and the heat treatment time is 90-120min; The vacuuming time in step 3 is 40-60 minutes.
9. The method for preparing a fabric according to claim 1, characterized in that: The following steps are involved: Step 1: After the polybutylene terephthalate fiber mesh cloth is rolled into a roll shape by a winder, it is immersed in the immersion liquid of the static sedimentation tank; Step 2: Take out the soaked mesh and squeeze out the excess soaking liquid in the embossing roller; Step 3: Put the mesh into the drying room for drying to obtain the desired fabric.
10. The method for preparing a fabric according to claim 9, characterized in that: In the step 1, the temperature of the soaking liquid is set to 30-40°C, and the soaking time is 20-30min; In step 3, the drying chamber temperature is set to 110-130°C, and the drying time is 40-60min; The weaving process of the polybutylene terephthalate fiber mesh cloth is one of warp knitting, stretch fabric and woven fabric; The immersion liquid includes resin, solvent and catalyst.
Citation Information
Patent Citations
High-tear-resistance and corrosion-resistance silicone rubber as well as preparation method and application thereof
CN104788965A
One-component addition type liquid silicone rubber and preparation method thereof
CN105238070A
Two-component bonding nylon silica gel and preparation method thereof
CN108929650A
Platinum vulcanization extrusion precipitation silicone rubber and preparation method thereof
CN113337124A
Solar energy silica -gel plate
CN207690804U