Anti-aging woven bag and preparation process thereof

By using the combination of polypropylene, phenolic resin and other materials in plastic woven bags, a stable crosslinking network and modified compounds are formed, which solves the problem of insufficient aging resistance performance of existing plastic woven bags, and realizes the high temperature and ultraviolet conditions. long-term stability and strength maintenance.

CN118931032AInactive Publication Date: 2024-11-12WENZHOU LONGQING PLASTIC IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410980128.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing plastic woven bags are prone to aging under direct sunlight and high temperature conditions, have short service life and insufficient aging resistance.

Method used

Using the combination of components such as polypropylene, phenolic resin, n-octyl boric acid, glycerin, nano-zinc oxide and ultraviolet absorbers, the formation of zinc compounds of n-octyl boric acid is combined with hydroxide Sodium-catalyzed silicon-oxygen bonds and Lewis acid-catalyzed glass fiber modifications improve the antioxidant and thermal properties of woven bags.

Benefits of technology

It significantly improves the aging resistance of woven bags, extends its service life, and can maintain high strength and stability under high temperature and ultraviolet irradiation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004955808000000101
    Figure BDA0004955808000000101
  • Figure BDA0004955808000000111
    Figure BDA0004955808000000111
  • Figure BDA0004955808000000121
    Figure BDA0004955808000000121
Patent Text Reader

Abstract

The invention relates to an anti-aging woven bag. The anti-aging woven bag comprises polypropylene, phenolic resin, n-octylboronic acid, glycerol, nano zinc oxide and an ultraviolet light absorber, the preparation technology of the anti-aging woven bag comprises the steps of raw material preparation and wiredrawing weaving. The invention has the following advantages and effects: the phenolic resin has a stable molecular structure and forms a three-dimensional cross-linked network after being cured, so that the phenolic resin has good aging resistance, and the woven bag prepared by blending the phenolic resin with the polypropylene containing the long saturated carbon chain can obtain a relatively high aging-resistant effect; according to the preparation method, n-octyl boric acid and glycerol react, namely hydroxyl in glycerol and boron atoms are coordinated to generate an intermediate compound, the intermediate compound further reacts with nano-zinc oxide, and the n-octyl boric acid monoglyceride zinc compound is obtained and assists in improving the performance of the woven bag, so that the woven bag shows good aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of woven bags, and in particular to an aging-resistant woven bag and a preparation process thereof. Background Art

[0002] High-quality plastic woven bags can be reused, reducing a lot of unnecessary waste of resources and environmental pollution. Under direct sunlight, the strength of plastic woven bags will decrease by 25% after one week and 40% after two weeks, and they are basically unusable. Existing plastic woven bags are prone to aging under high temperatures and ultraviolet rays in summer, and have a short service life.

[0003] In view of the above-mentioned related technologies, the inventor believes that the aging resistance of some current plastic woven bags still needs to be improved. Summary of the invention

[0004] In order to improve the aging resistance of plastic woven bags, the present application provides an aging-resistant woven bag and a preparation process thereof.

[0005] In the first aspect, the present application provides an anti-aging woven bag adopting the following technical solution:

[0006] An anti-aging woven bag comprises the following components in parts by weight:

[0007] 40-50 parts of polypropylene;

[0008] 7-9 parts of phenolic resin;

[0009] 8-10 parts of n-octylboric acid;

[0010] 6-9 parts glycerin;

[0011] 3-4 parts of nano zinc oxide;

[0012] 1-2 parts of UV absorber.

[0013] By adopting the above technical scheme, the phenolic resin has a stable molecular structure, forms a three-dimensional cross-linked network after curing, and thus has good aging resistance. The woven bag prepared by blending with polypropylene containing a long saturated carbon chain can obtain a higher aging resistance effect; through the reaction of n-octylboric acid and glycerol, that is, the hydroxyl group in glycerol coordinates with the boron atom to generate an intermediate compound, which further reacts with nano zinc oxide to obtain n-octylboric acid monoglyceride zinc compound, which assists in improving the performance of the woven bag and makes it show good aging resistance.

[0014] Preferably, by weight, the mixture further comprises 5-8 parts of 3-(tert-butyldimethylsilyloxy)glutaric anhydride and 0.4-0.5 parts of sodium hydroxide.

[0015] By adopting the above technical scheme, under the catalysis of sodium hydroxide, 3-(tert-butyldimethylsilyloxy)glutaric anhydride is added to modify the phenolic resin on the one hand, so that the molecules are connected through ester bonds, the antioxidant ability is enhanced, and the stability in high temperature and oxidative environment is improved; on the other hand, the silicon-oxygen bond is more stable than the carbon-carbon bond and has a high resistance to heat and oxidation. The silicon-oxygen bond segment is introduced into the modified phenolic resin to further improve the aging resistance of the component.

[0016] Preferably, by weight, it also includes 1-2 parts of glass fiber, 2-4 parts of n-caproic anhydride and 0.2-0.3 parts of TiCl4.

[0017] By adopting the above technical scheme, in the presence of Lewis acid catalyst TiCl4, the glass fiber is modified by n-hexanoic anhydride with a saturated carbon chain, and the anhydride groups of n-hexanoic anhydride interact with the silanol groups formed by the hydrolysis reaction between the glass fiber and water molecules in the air, so that the glass fiber is firmly oriented and adsorbed on the fiber, and stable saturated carbon-hydrogen bonds are introduced, which helps to improve the aging resistance; in addition, the silanol groups on the surface of the glass fiber can also react with the anhydride groups of 3-(tert-butyldimethylsiloxy)glutaric anhydride to form a stronger interface bond; at the same time, the catalyst TiCl4 can also catalyze the mutual reaction between n-hexanoic anhydride and 3-(tert-butyldimethylsiloxy)glutaric anhydride to form chemical bonds between the components, which, on the one hand, improves the interface bonding force between the glass fiber and other components, and on the other hand, is conducive to improving the overall antioxidant and aging resistance.

[0018] Preferably, in terms of weight ratio, the phenolic resin: 3-(tert-butyldimethylsilyloxy) glutaric anhydride: glass fiber: n-caproic anhydride = 7:6:1:3.

[0019] By adopting the above technical solution, a woven bag with better aging resistance can be obtained.

[0020] Preferably, the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole.

[0021] In the second aspect, the present application provides a preparation process for an aging-resistant woven bag, which adopts the following technical solution:

[0022] A preparation process of an aging-resistant woven bag comprises the following steps:

[0023] S1. Raw material preparation; n-octylboric acid and glycerol are mixed, stirred at 80-90°C for 2-3h, nano zinc oxide is added and stirred for 1-2h, then washed and filtered with anhydrous ethanol; polypropylene, phenolic resin and ultraviolet absorber are added and mixed to obtain raw materials;

[0024] S2. Wire drawing and weaving: the raw materials of S1 are put into the extruder, melted at 200-220℃, extruded and wire drawn, and then woven, cut and sewn into finished woven bags.

[0025] Preferably, the method further comprises the following steps: dissolving 7-9 parts of phenolic resin in 12-13 parts of ethanol, and then adding 4-6 parts of 3-(tert-butyldimethylsilyloxy)glutaric anhydride and 0.4-0.5 parts of sodium hydroxide, and stirring at 50-60° C. for 3-4 hours to obtain a mixture A;

[0026] 1-2 parts of glass fiber, 2-4 parts of n-hexanoic anhydride and 0.2-0.3 parts of TiCl4 are mixed, and ultrasonically dispersed at 30-40 KHz, 150-160 W for 5-6 minutes, and then the remaining 3-(tert-butyldimethylsilyloxy)glutaric anhydride is added and mixed, and the temperature is raised to 90-100° C. and stirred for 1-2 hours to obtain a mixture B;

[0027] 8-10 parts of n-octylboric acid and 6-9 parts of glycerol are blended, stirred at 80-90°C for 2-3 hours, then 3-4 parts of nano zinc oxide are added and stirred for 1-2 hours, then washed and filtered with anhydrous ethanol; then 40-50 parts of polypropylene, mixture A, mixture B and 1-2 parts of ultraviolet absorber are added and blended to obtain a raw material.

[0028] In summary, this application includes the following beneficial technical effects:

[0029] 1. Phenolic resin has a stable molecular structure. After curing, it forms a three-dimensional cross-linked network and has good aging resistance. The woven bag made by blending with polypropylene containing long saturated carbon chains can obtain a higher aging resistance effect. Through the reaction of n-octylboric acid and glycerol, the hydroxyl group in glycerol coordinates with the boron atom to generate an intermediate compound, which further reacts with nano zinc oxide to obtain n-octylboric acid monoglyceride zinc compound, which helps to improve the performance of the woven bag and makes it show good aging resistance.

[0030] 2. Under the catalysis of sodium hydroxide, 3-(tert-butyldimethylsilyloxy) glutaric anhydride is added to modify the phenolic resin on the one hand, so that the molecules are connected through ester bonds, the antioxidant capacity is enhanced, and the stability under high temperature and oxidative environment is improved; on the other hand, the silicon-oxygen bond is more stable than the carbon-carbon bond and has a high resistance to heat and oxidation. The silicon-oxygen bond segment is introduced into the modified phenolic resin to further improve the aging resistance of the component;

[0031] 3. In the presence of Lewis acid catalyst TiCl4, the glass fiber is modified by n-hexanoic anhydride with a saturated carbon chain. The anhydride groups of n-hexanoic anhydride interact with the silanol groups formed by the hydrolysis reaction of the glass fiber and water molecules in the air, and are firmly oriented and adsorbed on the fiber. At the same time, stable saturated carbon-hydrogen bonds are introduced, which helps to improve the aging resistance. In addition, the silanol groups on the surface of the glass fiber can also react with the anhydride groups of 3-(tert-butyldimethylsiloxy)glutaric anhydride to form a stronger interface bond. At the same time, the catalyst TiCl4 can also catalyze the mutual reaction between n-hexanoic anhydride and 3-(tert-butyldimethylsiloxy)glutaric anhydride to form chemical bonds between the components, which, on the one hand, improves the interface bonding force between the glass fiber and other components, and on the other hand, is conducive to improving the overall antioxidant and aging resistance. DETAILED DESCRIPTION

[0032] The present application is described in further detail below.

[0033] In the present application, polypropylene is provided by Shanghai Tuoxin Hongwei Plastic Raw Materials Co., Ltd., the manufacturer (origin) is Taiwan Formosa Plastics, brand 5090T; phenolic resin is thermosetting phenolic resin provided by Shandong Xujie Chemical Co., Ltd., CAS number: 9003-35-4; n-octylboric acid, CAS number: 28741-08-4; nano zinc oxide is 50nm grade provided by Hebei Teng Bimetallic Materials Co., Ltd.; 3-tert-butyldimethylsiloxyglutaric anhydride, CAS number: 91424-40-7; glass fiber is provided by Tai'an Zhongshuo Glass Fiber Products Co., Ltd., specification EMG10-35; n-hexanoic anhydride, CAS number: 2051-49-2; 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, CAS number: 2440-22-4.

[0034] Unless otherwise specified, the raw materials used in the following embodiments can be obtained from common commercial sources.

[0035] Example

[0036] Example 1

[0037] The present embodiment discloses an aging-resistant woven bag and a preparation process thereof; an aging-resistant woven bag, comprising the following components: polypropylene, phenolic resin, n-octylboric acid, glycerol, nano zinc oxide and ultraviolet absorber, wherein the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and the content of each component is shown in Table 1 below.

[0038] A preparation process of an aging-resistant woven bag comprises the following steps:

[0039] S1. Raw material preparation; n-octylboric acid and glycerol are mixed, stirred at 80°C for 2h, nano zinc oxide is added and stirred for 1h, then washed and filtered with anhydrous ethanol; polypropylene, phenolic resin and ultraviolet absorber are added and mixed to obtain a raw material;

[0040] S2. Wire drawing and weaving: the raw materials of S1 are put into the extruder, melted at 200℃, extruded and drawn to form flat wires, and then woven, cut and sewn into finished woven bags.

[0041] The infrared spectrum of the reaction product of n-octylboric acid, glycerol and nano zinc oxide was tested: at 1236 cm -1 and 1402cm -1 The stretching vibration band of monoglyceride of borate appears at 280 cm -1 is the stretching vibration absorption peak of CH, 551cm -1 The BO characteristic vibration absorption peak appears at , indicating the occurrence of the reaction.

[0042] Example 2

[0043] The present embodiment discloses an aging-resistant woven bag and a preparation process thereof; an aging-resistant woven bag, comprising the following components: polypropylene, phenolic resin, n-octylboric acid, glycerol, nano zinc oxide and ultraviolet absorber, wherein the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and the content of each component is shown in Table 1 below.

[0044] A preparation process of an aging-resistant woven bag comprises the following steps:

[0045] S1. Raw material preparation; n-octylboric acid and glycerol were mixed, stirred at 90°C for 3h, nano zinc oxide was added and stirred for 2h, then washed and filtered with anhydrous ethanol; polypropylene, phenolic resin and ultraviolet absorber were added and mixed to obtain a raw material;

[0046] S2. Wire drawing and weaving: the raw materials of S1 are put into the extruder, melted at 220℃, extruded and drawn to form flat wires, and then woven, cut and sewn into finished woven bags.

[0047] Example 3

[0048] The present embodiment discloses an aging-resistant woven bag and a preparation process thereof; an aging-resistant woven bag, comprising the following components: polypropylene, phenolic resin, n-octylboric acid, glycerol, nano zinc oxide and ultraviolet absorber, wherein the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and the content of each component is shown in Table 1 below.

[0049] A preparation process of an aging-resistant woven bag comprises the following steps:

[0050] S1. Raw material preparation; n-octylboric acid and glycerol were mixed, stirred at 85°C for 2.5h, nano zinc oxide was added and stirred for 1.5h, then washed and filtered with anhydrous ethanol; polypropylene, phenolic resin and ultraviolet absorber were added and mixed to obtain a raw material;

[0051] S2. Wire drawing and weaving: the raw materials of S1 are put into the extruder, melted at 210℃, extruded and drawn to form flat wires, and then woven, cut and sewn into finished woven bags.

[0052] Example 4

[0053] The difference from Example 1 is that an aging-resistant woven bag includes the following components: polypropylene, phenolic resin, n-octylboric acid, glycerol, nano zinc oxide, ultraviolet absorber, 3-(tert-butyldimethylsilyloxy)glutaric anhydride, sodium hydroxide, glass fiber, n-hexanoic anhydride and TiCl4, wherein the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and the content of each component is shown in Table 1 below.

[0054] A process for preparing an aging-resistant woven bag, S1 further comprising the following steps:

[0055] The phenolic resin was dissolved in 12 parts of ethanol, and then 4 parts of 3-(tert-butyldimethylsilyloxy)glutaric anhydride and sodium hydroxide were added and mixed, and stirred at 50° C. for 3 hours to obtain a mixture A;

[0056] The glass fiber, hexanoic anhydride and TiCl4 were mixed, and ultrasonically dispersed at 30KHz, 150W for 5min, and then the remaining 3-(tert-butyldimethylsilyloxy)glutaric anhydride was added and mixed, and the mixture was heated to 90°C and stirred for 1h to obtain a mixture B;

[0057] Octylboric acid and glycerol were mixed, stirred at 80° C. for 2 h, nano zinc oxide was added and stirred for 1 h, then washed and filtered with anhydrous ethanol; polypropylene, mixture A, mixture B and ultraviolet absorber were added and blended to obtain a raw material.

[0058] Example 5

[0059] The difference from Example 2 is that an aging-resistant woven bag includes the following components: polypropylene, phenolic resin, n-octylboric acid, glycerol, nano zinc oxide, ultraviolet absorber, 3-(tert-butyldimethylsilyloxy)glutaric anhydride, sodium hydroxide, glass fiber, n-hexanoic anhydride and TiCl4, wherein the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and the content of each component is shown in Table 1 below.

[0060] A process for preparing an aging-resistant woven bag, S1 further comprising the following steps:

[0061] The phenolic resin was dissolved in 13 parts of ethanol, and then 6 parts of 3-(tert-butyldimethylsilyloxy)glutaric anhydride and sodium hydroxide were added and mixed, and stirred at 60° C. for 4 hours to obtain a mixture A;

[0062] The glass fiber, hexanoic anhydride and TiCl4 were mixed, and ultrasonically dispersed at 40KHz, 160W for 6min, and then the remaining 3-(tert-butyldimethylsilyloxy)glutaric anhydride was added and mixed, and the mixture was heated to 100°C and stirred for 2h to obtain a mixture B;

[0063] Octylboric acid and glycerol are mixed, stirred at 90° C. for 3 hours, nano zinc oxide is added and stirred for 2 hours, then washed and filtered with anhydrous ethanol; polypropylene, mixture A, mixture B and ultraviolet absorber are added and blended to obtain a raw material.

[0064] Example 6

[0065] The difference from Example 3 is that an aging-resistant woven bag includes the following components: polypropylene, phenolic resin, n-octylboric acid, glycerol, nano zinc oxide, ultraviolet absorber, 3-(tert-butyldimethylsilyloxy)glutaric anhydride, sodium hydroxide, glass fiber, n-hexanoic anhydride and TiCl4, wherein the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and the content of each component is shown in Table 1 below.

[0066] A process for preparing an aging-resistant woven bag, S1 further comprising the following steps:

[0067] The phenolic resin was dissolved in 13 parts of ethanol, and then 5 parts of 3-(tert-butyldimethylsilyloxy)glutaric anhydride and sodium hydroxide were added and mixed, and stirred at 55° C. for 3.5 hours to obtain a mixture A;

[0068] The glass fiber, hexanoic anhydride and TiCl4 were mixed and dispersed ultrasonically at 35KHz and 155W for 6 minutes, and then the remaining 3-(tert-butyldimethylsilyloxy)glutaric anhydride was added and mixed, and the mixture was heated to 95°C and stirred for 1.5 hours to obtain a mixture B;

[0069] Octylboric acid and glycerol were mixed, stirred at 85° C. for 2.5 hours, nano zinc oxide was added, and stirring was continued for 1.5 hours, and then washed and filtered with anhydrous ethanol; polypropylene, mixture A, mixture B and ultraviolet absorber were added and blended to obtain a raw material.

[0070] Example 7

[0071] The difference from Example 1 is that the components of the aging-resistant woven bag also include 3-(tert-butyldimethylsilyloxy)glutaric anhydride and sodium hydroxide.

[0072] Example 8

[0073] The difference from Example 7 is that 3-(tert-butyldimethylsilyloxy)glutaric anhydride is replaced by phthalic anhydride.

[0074] Example 9

[0075] The difference from Example 4 is that the glass fiber is replaced by 800 mesh quartz powder.

[0076] Example 10

[0077] The difference from Example 9 is that n-hexanoic anhydride is replaced by maleic anhydride.

[0078] Embodiment 11

[0079] The difference from Example 10 is that TiCl4 is replaced by ZnCl2.

[0080] Example 12

[0081] The difference from Example 1 is that the ultraviolet absorber is ultraviolet absorber UV-531.

[0082] Embodiment 13

[0083] The difference from Example 4 is that, by weight ratio, phenolic resin: 3-(tert-butyldimethylsiloxy) glutaric anhydride: glass fiber: n-hexanoic anhydride = 7:6:1:3, i.e., 7 parts of phenolic resin, 6 parts of 3-(tert-butyldimethylsiloxy) glutaric anhydride, 1 part of glass fiber, and 3 parts of n-hexanoic anhydride.

[0084] Comparative Example

[0085] Comparative Example 1

[0086] The difference from Example 1 is that the phenolic resin is replaced by polycarbonate.

[0087] Comparative Example 2

[0088] The difference from Example 1 is that n-octylboronic acid is replaced by 5-ethylthiophene-2-boronic acid.

[0089] Comparative Example 3

[0090] The difference from Example 1 is that glycerol is replaced by ethanol.

[0091] Comparative Example 4

[0092] The difference from Example 1 is that nano zinc oxide is replaced by nano magnesium oxide.

[0093] Table 1 Component contents of Examples 1-6

[0094]

[0095] Performance testing

[0096] Test method: refer to the technical indicators and tests of flat yarn in GB / T 8946-2013, take 800mm of flat yarn samples prepared in each embodiment and comparative example, with a linear density of 109tex, a clamp spacing of 500mm, and an empty car descending speed of 300mm / min±2mm / min, until the sample breaks, and measure the maximum tensile load. Each sample is tested twice and the arithmetic mean is taken; relative tensile load = maximum tensile load / linear density, and the front relative tensile load value A1 of the flat yarn samples prepared in each embodiment and comparative example is measured;

[0097] Aging resistance test; The method in GB / T16422.3-1997 was used for detection. After the flat wire samples prepared in each embodiment and comparative example were exposed to UV-A fluorescent ultraviolet lamp for 4 hours, the relative tensile load A2 after aging was measured, and the relative tensile load retention rate = (relative tensile load value after aging A2 / previous relative tensile load A1) × 100%. The higher the retention rate, the better the tensile performance retention effect and the higher the aging resistance. The test results are shown in Table 2 below.

[0098] Table 2 Performance test results of various embodiments and comparative examples

[0099]

[0100]

[0101] (2) Tensile test: Take 20 500 mm flat wire samples with a linear density of 109 tex, a clamp spacing of 500 mm, and an empty vehicle lowering speed of 300 mm / min±2 mm / min until the sample breaks. The test results show that the tensile force of the flat wire is 703 N / 50 mm, which meets the requirement of 650 N / 50 mm specified in the national standard of "Plastic Woven Bags".

[0102] This specific implementation is merely an explanation of the present application and is not intended to limit the scope of protection of the present application. After reading this specification, those skilled in the art may make modifications to the present implementation as needed without any creative contribution, but as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. An anti-aging woven bag, characterized by: The composition comprises the following components in parts by weight: 40-50 parts of polypropylene; 7-9 parts of phenolic resin; 8-10 parts of n-octylboric acid; 6-9 parts glycerin; 3-4 parts of nano zinc oxide; 1-2 parts of UV absorber.

2. The anti-aging woven bag according to claim 1, characterized in that: By weight, the invention also includes 5-8 parts of 3-(tert-butyldimethylsilyloxy)glutaric anhydride and 0.4-0.5 parts of sodium hydroxide.

3. The anti-aging woven bag according to claim 2, characterized in that: By weight, it also includes 1-2 parts of glass fiber, 2-4 parts of n-caproic anhydride and 0.2-0.3 parts of TiCl4.

4. The anti-aging woven bag according to claim 3, characterized in that: In terms of weight ratio, the phenolic resin: 3-(tert-butyldimethylsilyloxy) glutaric anhydride: glass fiber: n-caproic anhydride = 7:6:1:

3.

5. The anti-aging woven bag according to claim 1, characterized in that: The ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole.

6. The process for preparing an anti-aging woven bag according to claim 1, characterized in that: The steps include: S1. Raw material preparation; n-octylboric acid and glycerol are mixed, stirred at 80-90°C for 2-3h, nano zinc oxide is added and stirred for 1-2h, then washed and filtered with anhydrous ethanol; polypropylene, phenolic resin and ultraviolet absorber are added and mixed to obtain raw materials; S2. Wire drawing and weaving: the raw materials of S1 are put into the extruder, melted at 200-220℃, extruded and drawn to form flat wires, and then woven, cut and sewn into finished woven bags.

7. The process for preparing an anti-aging woven bag according to claim 6, characterized in that: The method further comprises the following steps: dissolving 7-9 parts of phenolic resin in 12-13 parts of ethanol, and then adding 4-6 parts of 3-(tert-butyldimethylsilyloxy)glutaric anhydride and 0.4-0.5 parts of sodium hydroxide, and stirring at 50-60° C. for 3-4 hours to obtain a mixture A; 1-2 parts of glass fiber, 2-4 parts of n-hexanoic anhydride and 0.2-0.3 parts of TiCl4 are mixed, and ultrasonically dispersed at 30-40 KHz, 150-160 W for 5-6 minutes, and then the remaining 3-(tert-butyldimethylsilyloxy)glutaric anhydride is added and mixed, and the temperature is raised to 90-100° C. and stirred for 1-2 hours to obtain a mixture B; 8-10 parts of n-octylboric acid and 6-9 parts of glycerol are blended, stirred at 80-90°C for 2-3 hours, then 3-4 parts of nano zinc oxide are added and stirred for 1-2 hours, then washed and filtered with anhydrous ethanol; then 40-50 parts of polypropylene, mixture A, mixture B and 1-2 parts of ultraviolet absorber are added and blended to obtain a raw material.