Novel PVC coiled material fence for aquaculture
Through specific ratios of PVC resins and additives, the new PVC coil fence prepared solves the problems of the existing aquaculture fences, waterproof, moisture-proof and corrosion-resistant, and achieves efficient aquaculture environmental management and beautiful appearance. .
Patent Information
- Application Number
- CN202411179530.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
The existing aquaculture enclosure is not strong enough, has poor waterproof and moisture resistance, weak corrosion resistance, difficult cleaning, and monotonous appearance, resulting in increased breeding losses and difficult management.
The new PVC coil enclosure prepared by using PVC resin with specific ratios, impact modifiers, high temperature resistance, anti-aging agents and other raw materials, through high mixer stirring and extrusion plasticization technology, improve impact resistance and water resistance Moisture-proof performance and corrosion resistance, and prevent color fading through anti-aging agents to enhance appearance aesthetics.
It realizes long-term use of the fence, waterproof and moisture-proof effect, easy cleaning and maintenance, strong corrosion resistance, long-lasting and bright colors, beautiful appearance, reducing breeding costs and management difficulties.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of PVC coiled materials, and in particular to a novel PVC coiled material enclosure for aquaculture. Background Art
[0002] In aquaculture, in order to prevent escape from the breeding area, it is usually necessary to set up fences; however, ordinary aquaculture fences are not strong enough and are easily damaged when impacted by external forces. The waterproof and moisture-proof performance is relatively poor, which can easily cause moisture inside the fence and affect its use; the corrosion resistance is weak and it is easy to rust and corrode in harsh environments; it is difficult to clean, and the surface is prone to dust accumulation and stains, and it is not easy to clean; the appearance is relatively monotonous and not beautiful enough. These problems not only lead to losses in aquaculture, but also increase breeding costs and management difficulties. Therefore, it is of great practical significance to develop a fence that can solve the above problems. Summary of the invention
[0003] The purpose of the present invention is to provide a new type of PVC coil enclosure for aquaculture, which can effectively solve the technical problems mentioned in the background technology.
[0004] To achieve the above object, the present invention provides the following technical solutions: A new type of PVC coil enclosure for aquaculture is made of the following raw materials: The content of PVC resin is 100kg; Stabilizer 3-6kg; Calcium stearate 0.2-0.5kg; Impact modifier 4-8kg; Calcium carbonate 20kg; Lubricant 0.1-0.3kg; High temperature resistant agent 4-10kg; Anti-aging agent 2-8kg; Color powder 1-3kg; The preparation method of the novel PVC coil enclosure for aquaculture comprises the following steps: S1. Ingredients: Use an electronic scale to weigh the above raw material components separately: S2. Mixing: Pour the weighed PVC resin, stabilizer, calcium stearate, impact modifier, calcium carbonate, lubricant, high temperature resistant agent, anti-aging agent and color powder into a high-speed mixer in sequence, stir and mix thoroughly to ensure that all ingredients are evenly distributed; S3, extrusion plasticization: S31. Preheat the extrusion equipment 2 hours in advance; S32, start the equipment, closely observe the plasticization and demolding of the raw materials, and after the plasticization and demolding of the raw materials are uniform, accurately adjust the temperature to the specified range to ensure that the plasticization effect meets the requirements; S4, embossing process: When the temperature rises to between 160℃ - 220℃, start the production to ensure the quality and effect of embossing; S5, cooling and winding: S51. Slow down the equipment speed appropriately to ensure that the coil does not deform during the cooling process; S52. Accurately cut the coil and rewind it to ensure the neatness and tightness of the rewinding.
[0005] Preferably, the novel PVC coil enclosure for aquaculture is made of raw materials with the following weight ratio: The content of PVC resin is 100kg; Stabilizer 3-6kg; Calcium stearate 0.2-0.5kg; Impact modifier 8kg; Calcium carbonate 20kg; Lubricant 0.1-0.3kg; High temperature resistant agent 9kg; Anti-aging agent 2-8kg; Color powder 1-3kg.
[0006] Preferably, in step S2, the stirring temperature is 60°C and the stirring speed is 30 Hz.
[0007] Preferably, in step S4, the temperature of the calender is 190°C.
[0008] Compared with the prior art, the present invention has the following beneficial effects: The new PVC coil enclosure for aquaculture prepared by the present invention adds an impact modifier to improve processing performance, has good impact resistance and deformation resistance, and can be used for a long time; the added high temperature resistant agent is used to improve thermal stability, reduce thermal decomposition during processing and use, broaden the use temperature range, and has excellent high temperature resistance; the present invention has high-efficiency waterproof and moisture-proof properties, and can effectively prevent rainwater penetration from causing moisture inside the enclosure; it is easy to clean and maintain, has a smooth surface, and is not easily contaminated with dirt; it has strong corrosion resistance and is not corroded by chemical substances such as acids and alkalis; the anti-aging agent is used to inhibit oxidation reactions, absorb ultraviolet rays, and prevent the coil from fading, brittleness and other aging phenomena, which is conducive to long-lasting and bright colors, not easy to fade, and beautiful appearance. DETAILED DESCRIPTION
[0009] The technical solution of the present invention is described in detail below in conjunction with embodiments, but the protection scope is not limited thereto. Example
[0010] A new type of PVC coiled material enclosure for aquaculture is made of the following raw materials: 100kg of PVC resin, 5kg of stabilizer, 0.3kg of calcium stearate, 6kg of impact modifier, 20kg of calcium carbonate, 0.2kg of lubricant, 8kg of high temperature resistant agent, 6kg of anti-aging agent, and 2kg of color powder; wherein the PVC resin is polyvinyl chloride resin; The preparation method of the novel PVC coil enclosure for aquaculture comprises the following steps: S1. Ingredients: Use an electronic scale to weigh the above raw material components separately: S2. Mixing: Pour the weighed PVC resin, stabilizer, calcium stearate, impact modifier, calcium carbonate, lubricant, high temperature resistant agent, anti-aging agent and color powder into a high-speed mixer in sequence, stir and mix thoroughly to ensure that all ingredients are evenly distributed; S3, extrusion plasticization: S31. Preheat the extrusion equipment 2 hours in advance; S32, start the equipment, closely observe the plasticization and demolding of the raw materials, and after the plasticization and demolding of the raw materials are uniform, accurately adjust the temperature to the specified range to ensure that the plasticization effect meets the requirements; S4, embossing process: When the temperature rises to between 160℃ - 220℃, start the production to ensure the quality and effect of embossing; S5, cooling and winding: S51. Slow down the equipment speed appropriately to ensure that the coil does not deform during the cooling process; S52. Accurately cut the coil and rewind it to ensure the neatness and tightness of the rewinding. Example
[0011] A new type of PVC coiled material enclosure for aquaculture is made of the following raw materials: 100kg of PVC resin, 5kg of stabilizer, 0.3kg of calcium stearate, 8kg of impact modifier, 20kg of calcium carbonate, 0.2kg of lubricant, 8kg of high temperature resistant agent, 6kg of anti-aging agent, and 2kg of color powder; wherein the PVC resin is polyvinyl chloride resin; The preparation method of the novel PVC coil enclosure for aquaculture comprises the following steps: S1. Ingredients: Use an electronic scale to weigh the above raw material components separately: S2. Mixing: Pour the weighed PVC resin, stabilizer, calcium stearate, impact modifier, calcium carbonate, lubricant, high temperature resistant agent, anti-aging agent and color powder into a high-speed mixer in sequence, stir and mix thoroughly to ensure that all ingredients are evenly distributed; S3, extrusion plasticization: S31. Preheat the extrusion equipment 2 hours in advance; S32, start the equipment, closely observe the plasticization and demolding of the raw materials, and after the plasticization and demolding of the raw materials are uniform, accurately adjust the temperature to the specified range to ensure that the plasticization effect meets the requirements; S4, embossing process: When the temperature rises to between 160℃ - 220℃, start the production to ensure the quality and effect of embossing; S5, cooling and winding: S51. Slow down the equipment speed appropriately to ensure that the coil does not deform during the cooling process; S52. Accurately cut the coil and rewind it to ensure the neatness and tightness of the rewinding. Example
[0012] A new type of PVC coiled material enclosure for aquaculture is made of the following raw materials: 100kg of PVC resin, 5kg of stabilizer, 0.3kg of calcium stearate, 8kg of impact modifier, 20kg of calcium carbonate, 0.2kg of lubricant, 9kg of high temperature resistant agent, 6kg of anti-aging agent, and 2kg of color powder; wherein the PVC resin is polyvinyl chloride resin; The preparation method of the novel PVC coil enclosure for aquaculture comprises the following steps: S1. Ingredients: Use an electronic scale to weigh the above raw material components separately: S2. Mixing: Pour the weighed PVC resin, stabilizer, calcium stearate, impact modifier, calcium carbonate, lubricant, high temperature resistant agent, anti-aging agent and color powder into a high-speed mixer in sequence, stir and mix thoroughly to ensure that all ingredients are evenly distributed; S3, extrusion plasticization: S31. Preheat the extrusion equipment 2 hours in advance; S32, start the equipment, closely observe the plasticization and demolding of the raw materials, and after the plasticization and demolding of the raw materials are uniform, accurately adjust the temperature to the specified range to ensure that the plasticization effect meets the requirements; S4, embossing process: When the temperature rises to between 160℃ - 220℃, start the production to ensure the quality and effect of embossing; S5, cooling and winding: S51. Slow down the equipment speed appropriately to ensure that the coil does not deform during the cooling process; S52. Accurately cut the coil and rewind it to ensure the neatness and tightness of the rewinding. Example
[0013] A new type of PVC coiled material enclosure for aquaculture is made of the following raw materials: 100kg of PVC resin, 5kg of stabilizer, 0.3kg of calcium stearate, 8kg of impact modifier, 20kg of calcium carbonate, 0.2kg of lubricant, 9kg of high temperature resistant agent, 8kg of anti-aging agent, and 2kg of color powder; wherein the PVC resin is polyvinyl chloride resin; The preparation method of the novel PVC coil enclosure for aquaculture comprises the following steps: S1. Ingredients: Use an electronic scale to weigh the above raw material components separately: S2. Mixing: Pour the weighed PVC resin, stabilizer, calcium stearate, impact modifier, calcium carbonate, lubricant, high temperature resistant agent, anti-aging agent and color powder into a high-speed mixer in sequence, stir and mix thoroughly to ensure that all ingredients are evenly distributed; S3, extrusion plasticization: S31. Preheat the extrusion equipment 2 hours in advance; S32, start the equipment, closely observe the plasticization and demolding of the raw materials, and after the plasticization and demolding of the raw materials are uniform, accurately adjust the temperature to the specified range to ensure that the plasticization effect meets the requirements; S4, embossing process: When the temperature rises to between 160℃ - 220℃, start the production to ensure the quality and effect of embossing; S5, cooling and winding: S51. Slow down the equipment speed appropriately to ensure that the coil does not deform during the cooling process; S52. Cut the coil accurately and rewind the coil to ensure the neatness and tightness of the coil. Example
[0014] A new type of PVC coiled material enclosure for aquaculture is made of the following raw materials: 100kg of PVC resin, 5kg of stabilizer, 0.3kg of calcium stearate, 8kg of impact modifier, 20kg of calcium carbonate, 0.2kg of lubricant, 9kg of high temperature resistant agent, 8kg of anti-aging agent, and 2kg of color powder; wherein the PVC resin is polyvinyl chloride resin; The preparation method of the novel PVC coil enclosure for aquaculture comprises the following steps: S1. Ingredients: Use an electronic scale to weigh the above raw material components separately: S2. Mixing: Pour the weighed PVC resin, stabilizer, calcium stearate, impact modifier, calcium carbonate, lubricant, high temperature resistant agent, anti-aging agent and color powder into a high-speed mixer in sequence, stir and mix thoroughly to ensure that the ingredients are evenly distributed. The stirring temperature is 60°C and the stirring speed is 30Hz. S3, extrusion plasticization: S31. Preheat the extrusion equipment 2 hours in advance; S32, start the equipment, closely observe the plasticization and demolding of the raw materials, and after the plasticization and demolding of the raw materials are uniform, accurately adjust the temperature to the specified range to ensure that the plasticization effect meets the requirements; S4, embossing process: When the temperature rises to between 160℃ - 220℃, start the production to ensure the quality and effect of embossing; S5, cooling and winding: S51. Slow down the equipment speed appropriately to ensure that the coil does not deform during the cooling process; S52. Accurately cut the coil and rewind it to ensure the neatness and tightness of the rewinding. Example
[0015] A new type of PVC coiled material enclosure for aquaculture is made of the following raw materials: 100kg of PVC resin, 5kg of stabilizer, 0.3kg of calcium stearate, 8kg of impact modifier, 20kg of calcium carbonate, 0.2kg of lubricant, 9kg of high temperature resistant agent, 8kg of anti-aging agent, and 2kg of color powder; wherein the PVC resin is polyvinyl chloride resin; The preparation method of the novel PVC coil enclosure for aquaculture comprises the following steps: S1. Ingredients: Use an electronic scale to weigh the above raw material components separately: S2. Mixing: Pour the weighed PVC resin, stabilizer, calcium stearate, impact modifier, calcium carbonate, lubricant, high temperature resistant agent, anti-aging agent and color powder into a high-speed mixer in sequence, stir and mix thoroughly to ensure that the ingredients are evenly distributed. The stirring temperature is 60°C and the stirring speed is 30Hz. S3, extrusion plasticization: S31. Preheat the extrusion equipment 2 hours in advance; S32, start the equipment, closely observe the plasticization and demolding of the raw materials, and after the plasticization and demolding of the raw materials are uniform, accurately adjust the temperature to the specified range to ensure that the plasticization effect meets the requirements; S4, embossing process: When the temperature rises to between 160℃ - 220℃, start the production to ensure the quality and effect of embossing. The temperature of the calender is 190℃; S5, cooling and winding: S51. Slow down the equipment speed appropriately to ensure that the coil does not deform during the cooling process; S52. Accurately cut the coil and rewind it to ensure the neatness and tightness of the rewinding.
[0016] Control group Ordinary PVC coils currently available on the market were used as the experimental subjects for the control group; Performance experiment: 1. Tensile test: testing the tensile strength of the products in the above-mentioned embodiments 1 to 6 and the control group; 1. Electronic universal testing machine with precise loading and measuring system; 2. Measuring tools, such as rulers, vernier calipers, etc., used to measure the size of the specimen; Experimental samples: Take the products in the above-mentioned embodiments 1 to 5 and the control group, cut long-shaped samples of the same size and meeting the standard requirements, and the number of samples in each group shall be no less than 5; Experimental steps: 1. Sample preparation and measurement: Use tools such as cutters to prepare samples with accurate dimensions, and use measuring tools to measure the original gauge length of the sample and the width and thickness of the sample within the gauge length. The measurement accuracy should meet the requirements.
[0017] 2. Install the specimen: Clamp both ends of the specimen in the upper and lower fixtures of the testing machine, ensuring that the specimen is firmly clamped and well-aligned to avoid slippage or eccentric loading during loading; 3. Set experimental parameters: Set the stretching speed, experimental termination conditions (such as specimen fracture) and other parameters in the control software of the testing machine.
[0018] 4. Conduct tensile test: Start the testing machine and stretch the sample at the set speed. During the stretching process, the testing machine will automatically record the tensile force and the elongation of the sample.
[0019] 5. Record data: When the specimen breaks, the testing machine stops running and the maximum tensile force (tensile strength) and the gauge length elongation when the specimen breaks are recorded.
[0020] 6. Repeat the experiment: Perform the same tensile test on the remaining specimens to obtain sufficient data for statistical analysis.
[0021] 2. Ball pressure test: testing the ball pressure hardness of the products in the above-mentioned embodiments 1 to 6 and the control group; The test temperature is 65℃, the sample thickness should be at least 2.5mm, and the two sheets should be in close contact. Keep the oven and ball pressure gauge at the test temperature for 24 hours until thermal equilibrium is reached. Place the sample in the oven and make its upper surface horizontal. Press the ball pressure gauge (load 20±0.5N, pressure ball diameter 5mm) onto this surface. Take out the sample after 1 hour, and immerse the sample in 20±5℃ cold water within 10s and keep it for 6±2min. Take out the sample and wipe off the water marks. Take out the sample from the water and wipe off the water marks. Measure the indentation diameter within 3 minutes after taking the sample out of the water. The indentation diameter is qualified if it does not exceed 2mm; 3. High temperature resistance test: Set the temperature of the high temperature test chamber according to the experimental requirements and the expected use environment. Usually, the temperature is gradually increased for testing, for example, starting from 50°C, and increasing by a certain amount each time (such as 20°C) until the expected maximum temperature is reached. Put in the sample, and put the products in the above-mentioned Examples 1 to 6 and the control group steadily into the high temperature test chamber with the set temperature. At each set temperature, maintain a certain time (for example, 2 hours) to simulate long-term high temperature exposure; 4. Anti-aging test: Prepare an aging test chamber, and adjust and control the temperature, humidity, light, etc. Ensure that the performance of the test chamber is stable and calibrated and verified. Set the temperature, humidity, light intensity, time and other parameters of the aging test according to relevant standards or actual use environment. Aging conditions include high temperature, high humidity, ultraviolet radiation, etc. Place the products in Examples 1 to 6 and the control group evenly on the sample rack in the aging test chamber, ensuring that there is enough space between the samples to avoid mutual influence. Observe and test the samples regularly at the set time intervals. Record the changes in parameters such as temperature, humidity and light in the test chamber. After the prescribed aging time is over, take out the samples for performance testing and observe the changes in appearance (color, gloss, cracks, deformation, etc.).
[0022] Table 1 Performance test results data: Ordinary PVC coils are not strong enough as aquaculture enclosures and are easily damaged when impacted by external forces. They have relatively poor waterproof and moisture-proof properties, which can easily cause moisture inside the enclosure and affect its use. They have weak corrosion resistance and are prone to rust and corrosion in harsh environments. They are difficult to clean, with dust and stains easily accumulating on the surface, and are not easy to clean. Their appearance is relatively monotonous and not beautiful enough.
[0023] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A new type of PVC coil enclosure for aquaculture, characterized in that: It is made from the following raw materials: The content of PVC resin is 100kg; Stabilizer 3-6kg; Calcium stearate 0.2-0.5kg; Impact modifier 4-8kg; Calcium carbonate 20kg; Lubricant 0.1-0.3kg; High temperature resistant agent 4-10kg; Anti-aging agent 2-8kg; Color powder 1-3kg; The preparation method of the novel PVC coil enclosure for aquaculture comprises the following steps: S1. Ingredients: Use an electronic scale to weigh the above raw material components separately: S2. Mixing: Pour the weighed PVC resin, stabilizer, calcium stearate, impact modifier, calcium carbonate, lubricant, high temperature resistant agent, anti-aging agent and color powder into a high-speed mixer in sequence, stir and mix thoroughly to ensure that all ingredients are evenly distributed; S3, extrusion plasticization: S31. Preheat the extrusion equipment 2 hours in advance; S32, start the equipment, closely observe the plasticization and demolding of the raw materials, and after the plasticization and demolding of the raw materials are uniform, accurately adjust the temperature to the specified range to ensure that the plasticization effect meets the requirements; S4, embossing process: When the temperature rises to between 160℃ - 220℃, start the production to ensure the quality and effect of embossing; S5, cooling and winding: S51. Slow down the equipment speed appropriately to ensure that the coil does not deform during the cooling process; S52. Accurately cut the coil and rewind it to ensure the neatness and tightness of the rewinding.
2. The novel PVC coil enclosure for aquaculture according to claim 1 is characterized in that: It is made of the following raw materials in the following weight ratio: The content of PVC resin is 100kg; Stabilizer 3-6kg; Calcium stearate 0.2-0.5kg; Impact modifier 8kg; Calcium carbonate 20kg; Lubricant 0.1-0.3kg; High temperature resistant agent 9kg; Anti-aging agent 8kg; Color powder 1-3kg.
3. The novel PVC coil enclosure for aquaculture according to claim 1 is characterized in that: In step S2, the stirring temperature is 60°C and the stirring speed is 30 Hz.
4. The novel PVC coil enclosure for aquaculture according to claim 3 is characterized in that: In step S4, the temperature of the calender was 190°C.