Anti-static high-performance sealing gasket and preparation method thereof

By using carbon nanotube modified fluoroelastomer and oxidatively modified conductive carbon black in the sealing gasket, combined with ultrasonic dispersion and two-stage vulcanization technology, the problems of electrostatic accumulation and performance of traditional sealing gaskets are solved, and high-performance sealing gaskets are achieved The preparation of the product has excellent electrical conductivity, mechanical properties and aging resistance, and is suitable for complex industrial environments.

CN118931072APending Publication Date: 2024-11-12ZHENJIANG RUIHAO ENG PLASTIC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411183916.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional seals may accumulate static electricity during use, affecting the operation of the equipment. The flexibility and compression of existing anti-static seals decrease, and the effect of antistatic agents does not last, especially in high temperature and high humidity environments.

Method used

Carbon nanotube modified fluoroelastomer is used as the matrix material, combined with oxidized modified conductive carbon black, and through ultrasonic dispersion and oxidation modification technology, combined with two-stage vulcanization technology, we have prepared excellent conductivity, mechanical properties and aging resistance. High performance gasket.

Benefits of technology

It realizes stable anti-static performance and sealing performance under high temperature, high pressure and corrosive media environments, avoids warping and deformation, significantly improves tensile strength, elongation of break and wear resistance, and is suitable for high-demand industries. application.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an anti-static high-performance sealing gasket and a preparation method thereof. The sealing gasket is prepared from carbon nano tube modified fluororubber, oxidation modified conductive carbon black, dioctyl phthalate, a double-disulfide agent, an antioxidant, filler and a toughening agent. Through surface modification treatment on the carbon nanotubes and the conductive carbon black, the balance of high conductivity and mechanical strength of the material is realized. The preparation process comprises the steps of surface treatment of the carbon nanotubes, mixing modification of the fluororubber, material mixing and multi-step vulcanization treatment. Through inspection, the sealing gasket has excellent anti-static performance, excellent anti-aging performance and good processing performance, and is suitable for industrial application requiring high sealing performance and anti-static performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of preparation of sealing pads, and more particularly to an antistatic high-performance sealing pad and a preparation method thereof. Background Art

[0002] With the continuous development of industrial technology, sealing materials are increasingly used in various fields, especially in high-precision industries such as petrochemicals, electronics, and aerospace, where the performance of sealing materials plays a vital role in the normal operation of equipment. As a commonly used sealing material, gaskets are mainly used to prevent the leakage of liquids or gases and ensure the airtightness and stability of the system. However, traditional gaskets may generate static electricity accumulation during use, which may affect the operation of equipment or systems and may even cause serious accidents such as fires and explosions.

[0003] The research and development of antistatic sealing pads has become the key to solving the above problems. Existing antistatic sealing pads usually achieve antistatic function by adding conductive fillers or using antistatic agents in the material. However, these methods often have the following problems:

[0004] (1) Adding conductive fillers will affect the flexibility and compressibility of the gasket, thereby reducing its sealing performance. Excessive fillers may also cause the corrosion resistance and aging resistance of the gasket to decrease.

[0005] (2) Although antistatic agents can effectively reduce static electricity accumulation in the short term, their effect often gradually weakens over time. Especially under harsh working conditions such as high temperature and high humidity, antistatic agents are prone to failure and cannot provide continuous antistatic protection.

[0006] Therefore, there is an urgent need for a new type of sealing gasket that has both good antistatic performance and efficient sealing performance, and its preparation method should be simple and easy to use, suitable for industrial production. This sealing gasket not only needs to have excellent antistatic performance, but also should maintain stable physical and chemical properties under complex environments such as high temperature, high pressure, and corrosive media, so as to meet the needs of modern industry for high-performance sealing materials. Summary of the invention

[0007] In order to solve the deficiencies of the prior art, an antistatic high-performance sealing pad and a preparation method thereof are provided. The specific scheme is as follows:

[0008] The invention discloses an antistatic high-performance sealing gasket, which comprises the following components in percentage by mass: 60-70% of carbon nanotube modified fluororubber; 20-25% of oxidized modified conductive carbon black; 5-10% of dioctyl ester; 1-3% of disulfide agent; 0.5-1% of antioxidant; 0.5-1% of filler; and 1-3% of toughening agent.

[0009] Further, the steps of carbon nanotube modified fluororubber are as follows:

[0010] S1: The carbon nanotubes were ultrasonically treated in a mixed solution of concentrated nitric acid and concentrated sulfuric acid for 2 hours, then washed with deionized water until neutral, and dried in vacuum;

[0011] S2: weighing the surface-treated carbon nanotubes according to 1-3% of the total weight of the fluororubber, adding them into an ethanol or acetone solution, and ultrasonically dispersing them for 30 minutes to ensure uniform distribution of the carbon nanotubes in the solution;

[0012] S3: Knead the fluororubber on an open mixer, heat it to 160-180° C., slowly add the dispersed carbon nanotubes into the fluororubber, and continue kneading for 10-20 minutes to make the carbon nanotubes evenly distributed in the fluororubber matrix.

[0013] Furthermore, the conductive carbon black has a specific surface area of ​​≥1000m 2 / g, conductivity ≥10 -5 S / cm.

[0014] Furthermore, the step of oxidatively modifying the conductive carbon black is to stir the conductive carbon black in a 30% concentration hydrogen peroxide solution, with the reaction temperature controlled at 50-60° C. for 2-4 hours.

[0015] Furthermore, the antioxidant is one or a combination of 2,6-di-tert-butyl-4-methylphenol or tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0016] Furthermore, the toughening agent is one or a combination of polyvinyl butyral or ethylene-vinyl acetate copolymer.

[0017] Furthermore, the filler is fumed silica, the particle size of the fumed silica is 5 to 15 nm, and the specific surface area of ​​the fumed silica is 150 to 300 m 2 / g.

[0018] A method for preparing an antistatic high-performance sealing pad comprises the following steps:

[0019] S1: Prepare raw materials according to the mass percentage of carbon nanotube modified fluororubber, oxidized modified conductive carbon black, dioctyl ester, disulfide, antioxidant, fumed silica, and toughening agent;

[0020] S2: Preparation of carbon nanotube modified fluororubber;

[0021] S3: adding oxidatively modified conductive carbon black, fumed silica, antioxidant, and toughening agent to the carbon nanotube-modified fluororubber in sequence, and kneading at 160-180° C. for 5-15 minutes;

[0022] S4: Put the mixed material into a mold and vulcanize it at a temperature of 150-170° C. and a pressure of 10-20 MPa for 20-30 minutes to form a preliminary shape of the sealing gasket;

[0023] S5: performing secondary vulcanization on the initially formed sealing gasket at 150-160° C. for 12-24 hours to further improve the crosslinking density and mechanical properties of the material;

[0024] S6: The sealing gasket after secondary vulcanization is naturally cooled to below 30°C at room temperature. During the cooling process, the sealing gasket is kept flat to avoid warping and deformation. Finally, the sealing gasket is trimmed and surface treated to obtain the final product.

[0025] Beneficial effects:

[0026] (1) The present invention provides an antistatic high-performance sealing gasket, which uses carbon nanotube-modified fluororubber as a base material, and further enhances its conductivity and mechanical properties by introducing oxidatively modified conductive carbon black. The carbon nanotube-modified fluororubber not only gives the material excellent flexibility and heat resistance, but also significantly improves the tensile strength and elongation at break of the sealing gasket. The oxidatively modified conductive carbon black effectively reduces the volume resistivity, so that the sealing gasket has good antistatic properties. At the same time, this composite material also exhibits excellent wear resistance and aging resistance, and is suitable for high-demand industrial applications.

[0027] (2) In the process of dispersing carbon nanotubes and modifying conductive carbon black, ultrasonic dispersion and oxidation modification technology are used to effectively ensure the uniformity and consistency of the materials. A two-stage vulcanization process is adopted, which combines primary vulcanization with secondary vulcanization, which not only improves the cross-linking density and mechanical properties of the sealing gasket, but also improves its aging resistance and dimensional stability, effectively avoiding the warping and deformation problems that are prone to occur in traditional processes. DETAILED DESCRIPTION

[0028] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0029] Embodiment 1:

[0030] The preparation steps of an antistatic high-performance sealing pad are as follows:

[0031] Step 1: Preparation of carbon nanotube-modified fluororubber

[0032] 1.1 Carbon Nanotube Processing

[0033] 10 g of carbon nanotubes were added to a mixed solution of concentrated nitric acid and concentrated sulfuric acid (volume ratio 1:1, concentration of both 98%). Ultrasonic treatment was performed in an ultrasonic processor for 2 hours to ensure that the surface of the carbon nanotubes was fully oxidized. After treatment, the carbon nanotubes were repeatedly washed with deionized water until the pH value of the solution reached neutral. The washed carbon nanotubes were vacuum dried at 60°C for 12 hours.

[0034] 1.2 Carbon Nanotube Dispersion

[0035] The treated carbon nanotubes were weighed to 2% of the total weight of the fluororubber, i.e., 2 grams, and added to 100 milliliters of ethanol and ultrasonically dispersed in an ultrasonic processor for 30 minutes to ensure that the carbon nanotubes were evenly dispersed.

[0036] 1.3. Mixing carbon nanotubes and fluororubber

[0037] Take 100 g of fluororubber, put it into an open mill, and mix it at 170° C. Slowly add the dispersed carbon nanotubes into the fluororubber and continue mixing for 15 minutes to ensure that the carbon nanotubes are evenly distributed in the fluororubber matrix.

[0038] Step 2: Prepare the gasket mixture

[0039] 2.1. Oxidation-modified conductive carbon black

[0040] 30 g of conductive carbon black was added to 500 ml of 30% hydrogen peroxide solution. Stirring was performed at 50°C for 3 hours to complete the oxidative modification. Afterwards, the conductive carbon black was separated by suction filtration and repeatedly washed with deionized water until the hydrogen peroxide was completely removed. The treated conductive carbon black was vacuum dried at 60°C for 12 hours.

[0041] 2.2. Mixing

[0042] The carbon nanotube modified fluororubber prepared above, 25 g of oxidized modified conductive carbon black, 7 g of dioctyl ester, 2 g of disulfide agent, 0.75 g of antioxidant, 1 g of fumed silica and 2 g of toughening agent were added into a mixer in sequence according to mass percentage, and mixed at 170°C for 10 minutes until the components were evenly distributed.

[0043] Step 3: Vulcanization

[0044] 3.1. Initial vulcanization

[0045] The mixed material is placed in a mold and vulcanized at 160°C and 15MPa pressure for 25 minutes to form the initial shape of the gasket.

[0046] 3.2. Secondary vulcanization

[0047] The initially formed sealing gasket was subjected to secondary vulcanization at 155°C for 20 hours to improve the crosslinking density and mechanical properties of the material.

[0048] 3.3. Cooling and trimming

[0049] The gasket after secondary vulcanization is naturally cooled to below 30°C at room temperature, and the gasket is kept flat during the cooling process to avoid warping and deformation. Finally, the gasket is trimmed and surface treated to obtain the final product.

[0050] Embodiment 2:

[0051] The preparation steps of an antistatic high-performance sealing pad are as follows:

[0052] Step 1: Preparation of carbon nanotube-modified fluororubber

[0053] 1.1. Carbon nanotube processing

[0054] 12 grams of carbon nanotubes were added to a mixed solution of concentrated nitric acid and concentrated sulfuric acid at a volume ratio of 1:1, with a concentration of 98%. Ultrasonic treatment was performed in an ultrasonic processor for 2 hours, and then washed with deionized water until neutral. The washed carbon nanotubes were vacuum dried at 60°C for 12 hours.

[0055] 1.2. Carbon nanotube dispersion

[0056] The treated carbon nanotubes were weighed at 2.5% of the total weight of the fluororubber, that is, 2.5 g, and added to 100 ml of ethanol for ultrasonic dispersion for 30 minutes.

[0057] 1.3. Mixing carbon nanotubes and fluororubber

[0058] Take 100 g of fluororubber, knead it at 170°C, add the dispersed carbon nanotubes, and mix for 20 minutes to make them evenly distributed.

[0059] Step 2: Prepare the gasket mixture

[0060] 2.1. Oxidation-modified conductive carbon black

[0061] 30 g of conductive carbon black was added to 500 ml of 30% hydrogen peroxide solution and stirred at 55° C. for 4 hours. Afterwards, it was washed with deionized water to remove the residual hydrogen peroxide and vacuum dried at 65° C. for 12 hours.

[0062] 2.2. Mixing

[0063] Add carbon nanotube modified fluororubber, 24 g oxidized modified conductive carbon black, 8 g dioctyl ester, 2.5 g disulfide, 1 g antioxidant, 1 g fumed silica and 3 g toughening agent into a mixer according to mass percentage and mix for 12 minutes.

[0064] Step 3: Vulcanization

[0065] 3.1. Initial vulcanization

[0066] Vulcanization was carried out at 165°C and 20 MPa pressure for 30 minutes.

[0067] 3.2. Secondary vulcanization

[0068] The secondary vulcanization was carried out at 160°C for 24 hours.

[0069] 3.3. Cooling and trimming

[0070] The sealing gasket is cooled to below 30°C and finally trimmed and surface treated.

[0071] Embodiment 3:

[0072] Step 1: Preparation of carbon nanotube-modified fluororubber

[0073] 1.1. Carbon nanotube processing

[0074] 15 g of carbon nanotubes were added into a mixed solution of concentrated nitric acid and concentrated sulfuric acid (volume ratio 1:1).

[0075] After ultrasonic treatment for 2 hours, the sample was washed with deionized water until neutral and then dried under vacuum at 60°C for 12 hours.

[0076] 1.2. Carbon nanotube dispersion

[0077] The treated carbon nanotubes were weighed at 3% of the total weight of the fluororubber, that is, 3 grams, and added to 100 ml of acetone for ultrasonic dispersion for 30 minutes.

[0078] 1.3. Mixing carbon nanotubes and fluororubber

[0079] Take 100 g of fluororubber, mix it at 175°C, add the dispersed carbon nanotubes, and mix for 20 minutes to make them evenly distributed.

[0080] Step 2: Prepare the gasket mixture

[0081] 2.1. Oxidation-modified conductive carbon black

[0082] 35 g of conductive carbon black was added to 500 ml of 30% hydrogen peroxide solution and stirred at 60° C. for 4 hours.

[0083] The samples were washed with deionized water to remove residual hydrogen peroxide and dried under vacuum at 70 °C for 12 h.

[0084] 2.2. Mixing

[0085] Add carbon nanotube modified fluororubber, 25 g of oxidized modified conductive carbon black, 9 g of dioctyl ester, 3 g of disulfide, 0.5 g of antioxidant, 1 g of fumed silica and 2 g of toughening agent into a mixer according to mass percentage and mix for 15 minutes.

[0086] Step 3: Vulcanization

[0087] 3.1. Initial vulcanization

[0088] Vulcanization was carried out at 170°C and 18 MPa pressure for 28 minutes.

[0089] 3.2. Secondary vulcanization

[0090] The secondary vulcanization was carried out at 155°C for 18 hours.

[0091] 3.3. Cooling and trimming

[0092] After cooling to below 30°C, trimming and surface treatment are performed to obtain the final product.

[0093] Comparative Example:

[0094] Traditional gasket

[0095] The sealing gaskets obtained in Examples 1 to 3 and the sealing gaskets of the comparative example were tested for performance, and the test results are as follows:

[0096] Test content Comparative Example Example 1 Example 2 Example 3 Volume resistivity (Ω·cm) <![CDATA[10 5 ]]> <![CDATA[10 3 ]]> <![CDATA[10 2 ]]> <![CDATA[10 2 ]]> Tensile strength(MPa) 12.0 15.5 16.0 16.3 Elongation at break (%) 150 180 185 190 Tear strength (kN / m) 30 40 42 45 Tensile strength retention after thermal aging (%) 75 85 88 90 Elongation retention after heat aging (%) 60 75 80 82

[0097] From the data in the above table, it can be seen that the sealing gasket in the embodiment shows a significantly lower volume resistivity, indicating that it has better conductivity and is suitable for anti-static applications. The tensile strength of the sealing gasket in the embodiment is significantly better than that of the traditional sealing gasket, showing stronger mechanical properties. The sealing gasket in the embodiment shows higher flexibility and ductility in elongation at break. The sealing gasket in the embodiment has a higher tear strength, which means that it is not easy to tear in actual use and is more durable. The tensile strength and elongation retention rate of the sealing gasket in the embodiment after heat aging are higher than those of the traditional sealing gasket, showing better aging resistance.

[0098] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An anti-static high-performance sealing pad, It is characterized in that The high-performance sealing gasket comprises the following components in percentage by mass: 60-70% carbon nanotube modified fluororubber; 20-25% oxidized modified conductive carbon black; 5-10% dioctyl ester; 1-3% disulfide agent; 0.5-1% antioxidant; 0.5-1% filler; and 1-3% toughening agent.

2. The antistatic high-performance sealing pad according to claim 1, It is characterized in that The steps of carbon nanotube modified fluororubber are as follows: S1: The carbon nanotubes were ultrasonically treated in a mixed solution of concentrated nitric acid and concentrated sulfuric acid for 2 hours, then washed with deionized water until neutral, and dried in vacuum; S2: weighing the surface-treated carbon nanotubes according to 1-3% of the total weight of the fluororubber, adding them into an ethanol or acetone solution, and ultrasonically dispersing them for 30 minutes to ensure uniform distribution of the carbon nanotubes in the solution; S3: Knead the fluororubber on an open mixer, heat it to 160-180° C., slowly add the dispersed carbon nanotubes into the fluororubber, and continue kneading for 10-20 minutes to make the carbon nanotubes evenly distributed in the fluororubber matrix.

3. The antistatic high-performance sealing pad according to claim 1, It is characterized in that The conductive carbon black has a specific surface area of ​​≥1000m 2 / g, conductivity ≥10 -5 S / cm.

4. The antistatic high-performance sealing pad according to claim 1, It is characterized in that The step of oxidatively modifying the conductive carbon black is to stir the conductive carbon black in a 30% concentration hydrogen peroxide solution for reaction, the reaction temperature is controlled at 50-60° C., and the reaction time is 2-4 hours.

5. The antistatic high-performance sealing pad according to claim 1, It is characterized in that The antioxidant is one or a combination of 2,6-di-tert-butyl-4-methylphenol or tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.

6. The antistatic high-performance sealing pad according to claim 1, It is characterized in that The toughening agent is one of polyvinyl butyral and ethylene-vinyl acetate copolymer or a combination of the two.

7. The antistatic high-performance sealing pad according to claim 1, It is characterized in that The filler is fumed silica, the particle size of which is 5 to 15 nm, and the specific surface area of ​​which is 150 to 300 m 2 / g.

8. A method for preparing an anti-static high-performance sealing pad, It is characterized in that The following steps are involved: S1: Prepare raw materials according to the mass percentage of carbon nanotube modified fluororubber, oxidized modified conductive carbon black, dioctyl ester, disulfide, antioxidant, fumed silica, and toughening agent; S2: Preparation of carbon nanotube modified fluororubber; S3: adding oxidatively modified conductive carbon black, fumed silica, antioxidant, and toughening agent to the carbon nanotube-modified fluororubber in sequence, and kneading at 160-180° C. for 5-15 minutes; S4: putting the mixed material into a mold and vulcanizing it at a temperature of 150-170° C. and a pressure of 10-20 MPa for 20-30 minutes to form a preliminary shape of the sealing gasket; S5: performing secondary vulcanization on the initially formed sealing gasket at 150-160° C. for 12-24 hours to further improve the crosslinking density and mechanical properties of the material; S6: The sealing gasket after secondary vulcanization is naturally cooled to below 30°C at room temperature. During the cooling process, the sealing gasket is kept flat to avoid warping and deformation. Finally, the sealing gasket is trimmed and surface treated to obtain the final product.

Citation Information

Cited By

  • Antistatic perfluoroether rubber composition and method for producing the same