Light guide master batch and preparation method thereof

Through the dispersion polymerization of modified BaSO4 microspheres and polystyrene, the PS@BaSO4 core-shell structure is formed, which solves the problems of high light loss and high mechanical processing accuracy requirements in traditional light guide plate manufacturing, and achieves high light efficiency and high uniformity Light guide performance, suitable for various molding methods.

CN118931079AInactive Publication Date: 2024-11-12FOSHAN XINRONG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193981.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional light guide plate manufacturing technology has problems such as high cost, high light loss, high mechanical processing accuracy requirements, poor replication stability and inability to adjust the light guide size, and requires a thicker diffusion film to ensure brightness uniformity.

Method used

Modified BaSO4 microspheres are used as light scattering factor, and the surface of the surface is changed from hydrophilic to hydrophobicity through silane coupling agent, forming a PS@BaSO4 core-shell structure, combined with polystyrene for dispersion polymerization, and improving dispersion and optical performance, realize multiple refraction, reflection and scattering of light, and improve the utilization and uniformity of light.

Benefits of technology

It achieves high light efficiency and high uniformity light guiding performance, reduces light loss, avoids the need to use thicker diffusion films, and has good material stability and dispersion, which is suitable for various molding methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015833130000081
    Figure BDA0005015833130000081
  • Figure BDA0005015833130000091
    Figure BDA0005015833130000091
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer material preparation, in particular to a light guide master batch and a preparation method thereof. The light guide master batch comprises the following raw material components in parts by weight: 60-80 parts of a resin base material, 5-15 parts of PS and BaSO4 microspheres and 1-6 parts of a dispersing agent, the PS and BaSO4 microspheres are prepared by using modified BaSO4 microspheres modified by a silane coupling agent as growth sites and dispersing, polymerizing and wrapping polystyrene on the surfaces of the modified BaSO4 microspheres. Compared with the prior art, the light guide master batch provided by the invention is added with the PS and BaSO4 microspheres, and when light passes through the light guide master batch, the light can be refracted and reflected for many times, so that the light becomes softer and more uniform, the light range is expanded, the uniformity is good, the luminous efficiency is high, the dispersity and compatibility of each component are good, and a product has excellent light guide performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer material preparation, and in particular to a light-guiding masterbatch and a preparation method thereof. Background Art

[0002] The light guide plate is a key component of the backlight module and light output. The brightness and uniformity of the backlight module depend on the design and manufacture of the light guide plate. Usually, the light guide plate has a micro-optical pattern to change the direction of light propagation. In traditional designs, the light guide plate has a specific pattern of dots on the bottom surface, where the dot pattern is used to diffuse the incident light from the light source over a wide angle to maintain uniform brightness over the entire display area. Manufacturing technologies for making dots include V-cutting, injection molding, laser etching, hot stamping, screen printing, etc. V-cutting, injection molding, and hot stamping require expensive molds, which lead to longer cycles and high costs. The screen-printed light guide plate has a large scattering angle and high brightness contrast of the printed dots, which will reduce the brightness of the light-emitting surface, resulting in greater light loss. In order to make the light evenly emitted, a thicker diffusion film must be used to correct the direction and uniformity of the light source, and the screen printing process has the problem of polluting the environment. Laser etching will damage the material of the light guide plate and affect aging resistance. The line structure of the roller-pressed structure dots has high requirements for mechanical processing accuracy, and the replication stability has deviations, and the light guide size is fixed and cannot be adjusted. Therefore, it is of great significance to study a light guide material that can effectively transmit light without a diffusion film, ensure brightness uniformity and light utilization. Summary of the invention

[0003] In view of this, the present invention provides a light-guiding masterbatch and a preparation method thereof, wherein the light-guiding masterbatch can achieve both high light efficiency and high uniformity.

[0004] In a first aspect, the present invention provides a light-guiding masterbatch, comprising the following raw material components in parts by weight: 60-80 parts of a resin base material, 5-15 parts of PS@BaSO4 microspheres, and 1-6 parts of a dispersant;

[0005] The PS@BaSO4 microspheres are prepared by using modified BaSO4 microspheres modified by a silane coupling agent as growth sites and by dispersing and polymerizing polystyrene on the surface of the microspheres.

[0006] BaSO4 has a high refractive index and can act as a scattering factor to scatter light when passing through, thereby enhancing the scattering performance of forward light and improving the haze of the material. However, it will seriously damage the light transmittance of the material, causing large light loss, which is not conducive to the application in the optical field, and has poor compatibility with commonly used organic substrates, affecting the performance of the material. The present invention uses a silane coupling agent to modify BaSO4, so that the surface performance of nano BaSO4 is changed from hydrophilic to hydrophobic, thereby improving the affinity of inorganic powder and organic matrix, and the silane coupling agent forms a protective layer on the surface of nano BaSO4, generating a steric hindrance effect, hindering the aggregation between nano particles, thereby improving the dispersibility of nano BaSO4; at the same time, the hydrophobically modified BaSO4 increases the adsorption with oily monomers, so that subsequent polystyrene can be better attached to its surface, and because the surface carries silane groups, it can be bonded with styrene monomers, making the PS@BaSO4 core-shell structure more solid.

[0007] The light-guiding masterbatch of the present invention is added with PS@BaSO4 microspheres, which use the modified BaSO4 core as the growth site to disperse and polymerize the growth of PS, and the PS shell acts as a light scattering factor with a similar scattering mode in the light path. Through the continuous refraction and scattering of light, the diffusion range of light is increased to the maximum extent while retaining the intensity of light, thereby improving the utilization rate of light energy and reducing light loss. And due to the difference in refractive index between PS and BaSO4, a double refraction screen of PS / BaSO4 is formed. When light passes through each PS@BaSO4 core-shell microsphere, it will be refracted, reflected and scattered multiple times inside, and the path of light has changed, optimizing the directivity of light, thereby achieving the improvement of light-guiding performance. The PS@BaSO4 core-shell microspheres provided by the present invention combine the advantages of high haze of inorganic nanoparticles, high transparency of organic microspheres, good compatibility with substrates, and uniform dispersion. The prepared light-guiding masterbatch can simultaneously meet the requirements of transparency, hue, hue stability, extrusion stability, and dimensional stability.

[0008] The light guide masterbatch of the present invention can be used to obtain a molded product by various molding methods according to the purpose, such as injection molding, extrusion molding, compression molding, blow molding, etc., and can be used as an optical component for transmitting light inside a molded product such as a light guide plate. The light guide plate processed from the molded product has good stability, high brightness, high light efficiency and high uniformity. The light guide masterbatch material can effectively guide light to the light-emitting surface, and the uniformity of light can be improved without using a thick diffusion film.

[0009] Optionally, the preparation method of the PS@BaSO4 microspheres comprises the following steps:

[0010] Step S1, adding barium sulfate and a silane coupling agent into deionized water, stirring and reacting for 1-3 hours, centrifuging, washing, and drying to obtain the modified BaSO4 microspheres;

[0011] Step S2, the modified BaSO4 microspheres, stabilizer polyvinyl pyrrolidone, anhydrous ethanol and deionized water are mixed evenly, styrene and initiator 2,2-azobisisobutyronitrile are added dropwise at 55-65°C, and then the temperature is raised to 70-80°C, and the reaction is carried out under nitrogen protection for 16-24 hours. After the product is cooled to room temperature, it is centrifuged, washed and dried to obtain the PS@BaSO4 microspheres.

[0012] Optionally, the silane coupling agent is selected from at least one of 3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane or 3-mercaptopropyltriethoxysilane.

[0013] Optionally, in step S1, the mass ratio of the barium sulfate to the silane coupling agent is 1:0.05-0.3.

[0014] Optionally, in step S2, the mass ratio of the modified BaSO4 microspheres, polyvinyl pyrrolidone, styrene, 2,2-azobisisobutyronitrile, anhydrous ethanol and deionized water is 2-4:0.4-0.6:10:0.1:80-90:10-20.

[0015] Optionally, the dispersant is selected from at least one of polyacrylamide, polyethylene wax, calcium stearate or hexenyl bisstearamide.

[0016] Optionally, the resin substrate is selected from at least one of polycarbonate, polymethyl methacrylate or polystyrene.

[0017] In a second aspect, the present invention also provides a method for preparing the above-mentioned light-guiding masterbatch, the preparation method comprising the following steps:

[0018] The raw material components are weighed according to the ratio, and the resin substrate, PS@BaSO4 microspheres and dispersant are evenly mixed, and then melt-blended in a twin-screw extruder, extruded and granulated to obtain the light-guiding masterbatch.

[0019] In a third aspect, the present invention also provides the use of the above-mentioned light-guiding masterbatch in the preparation of light-guiding plates and light-guiding films.

[0020] Optionally, the light-guiding masterbatch is added in an amount of 1wt%-20wt% to the light-guiding plate material.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The light-guiding masterbatch provided by the present invention is added with PS@BaSO4 microspheres, which combine the high light transmittance of the organic light diffuser with the high haze of the inorganic light diffuser. When the light passes through, multiple refractions and reflections may occur, thereby making the light softer and more uniform, expanding the range of light, and effectively guiding the light to the light-emitting surface without a diffusion film, and has good uniformity, high luminous efficiency, good dispersibility and compatibility of each component, so that the product has better physical parameters and comprehensive performance. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. Unless otherwise defined, all professional terms used hereinafter are the same as those skilled in the art generally understand. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the various reagents and raw materials used in the present invention are all commodities that can be purchased from the market or products that can be prepared by known methods.

[0024] In order to better illustrate the present invention, further examples are given below.

[0025] Example 1

[0026] This embodiment provides a light-guiding masterbatch, comprising the following raw material components in parts by weight: 70 parts of polymethyl methacrylate, 12 parts of PS@BaSO4 microspheres and 4 parts of polyethylene wax.

[0027] The above-mentioned light-guiding masterbatch is prepared by the following method:

[0028] Step S1, adding barium sulfate with a particle size of 40 nm and γ-aminopropylmethyldiethoxysilane in a mass ratio of 1:0.2 to deionized water, stirring mechanically at 300 rpm for 2 hours, centrifuging at 5000 rpm for 30 minutes, washing the centrifuged product with deionized water for 3 times, and vacuum drying at 60° C. for 12 hours to obtain the modified BaSO4 microspheres;

[0029] Step S2, 3 g of the modified BaSO4 microspheres, 0.5 g of stabilizer polyvinyl pyrrolidone, 80 g of anhydrous ethanol and 20 g of deionized water are mixed evenly, the temperature is raised to 60°C, 10 g of styrene and 0.1 g of initiator 2,2-azobisisobutyronitrile are slowly added dropwise, and then the temperature is raised to 75°C, and the reaction is carried out under nitrogen protection for 18 hours. After the product is cooled to room temperature, it is centrifuged at 8000 rpm in a high-speed centrifuge for 30 minutes, and the centrifuged product is washed 3 times with anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain the PS@BaSO4 microspheres;

[0030] Step S3, weigh polymethyl methacrylate, mix it with PS@BaSO4 microspheres and polyethylene wax evenly, and place it in a twin-screw extruder, set the head temperature to 240°C, the screw speed to 200r / min, extrude and granulate, and obtain the light-guiding masterbatch.

[0031] Example 2

[0032] This embodiment provides a light-guiding masterbatch, comprising the following raw material components in parts by weight: 75 parts of polymethyl methacrylate, 15 parts of PS@BaSO4 microspheres and 6 parts of polyethylene wax.

[0033] The above-mentioned light-guiding masterbatch is prepared by the following method:

[0034] Step S1, adding barium sulfate with a particle size of 40 nm and 3-aminopropyltriethoxysilane in a mass ratio of 1:0.3 to deionized water, stirring mechanically at 300 rpm for 3 hours, centrifuging at 5000 rpm for 30 minutes, washing the centrifuged product with deionized water for 3 times, and vacuum drying at 60° C. for 12 hours to obtain the modified BaSO4 microspheres;

[0035] Step S2, 4 g of the modified BaSO4 microspheres, 0.6 g of stabilizer polyvinyl pyrrolidone, 80 g of anhydrous ethanol and 20 g of deionized water are mixed evenly, the temperature is raised to 65°C, 10 g of styrene and 0.1 g of initiator 2,2-azobisisobutyronitrile are slowly added dropwise, and then the temperature is raised to 80°C, and the reaction is carried out under nitrogen protection for 24 hours. After the product is cooled to room temperature, it is centrifuged at 8000 rpm in a high-speed centrifuge for 30 minutes, and the centrifuged product is washed 3 times with anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain the PS@BaSO4 microspheres;

[0036] Step S3, weigh polymethyl methacrylate, mix it with PS@BaSO4 microspheres and polyethylene wax evenly, and place it in a twin-screw extruder, set the head temperature to 240°C, the screw speed to 200r / min, extrude and granulate, and obtain the light-guiding masterbatch.

[0037] Example 3

[0038] This embodiment provides a light-guiding masterbatch, comprising the following raw material components in parts by weight: 60 parts of polymethyl methacrylate, 10 parts of PS@BaSO4 microspheres and 3 parts of polyacrylamide.

[0039] The above-mentioned light-guiding masterbatch is prepared by the following method:

[0040] Step S1, adding barium sulfate with a particle size of 40 nm and γ-aminopropyltrimethoxysilane in a mass ratio of 1:0.05 to deionized water, stirring mechanically at 300 rpm for 1 hour, centrifuging at 5000 rpm for 30 minutes, washing the centrifuged product with deionized water for 3 times, and vacuum drying at 60° C. for 12 hours to obtain the modified BaSO4 microspheres;

[0041] Step S2, 2g of the modified BaSO4 microspheres, 0.4g of stabilizer polyvinyl pyrrolidone, 90g of anhydrous ethanol and 10g of deionized water are mixed evenly, the temperature is raised to 55°C, 10g of styrene and 0.1g of initiator 2,2-azobisisobutyronitrile are slowly added dropwise, and then the temperature is raised to 70°C, and the reaction is carried out under nitrogen protection for 16h. After the product is cooled to room temperature, it is centrifuged at 8000rpm in a high-speed centrifuge for 30min, and the centrifuged product is washed 3 times with anhydrous ethanol, and vacuum dried at 60°C for 12h to obtain the PS@BaSO4 microspheres;

[0042] Step S3, weigh polystyrene, mix it with PS@BaSO4 microspheres and polyacrylamide, and place it in a twin-screw extruder, set the head temperature to 230° C., the screw speed to 200 r / min, extrude and granulate to obtain the light-guiding masterbatch.

[0043] Comparative Example 1

[0044] This comparative example provides a light-guiding masterbatch, comprising the following raw material components in parts by weight: 70 parts of polymethyl methacrylate, 12 parts of modified BaSO4 microspheres and 4 parts of polyethylene wax.

[0045] The above-mentioned light-guiding masterbatch is prepared by the following method:

[0046] Step S1, adding barium sulfate with a particle size of 40 nm and γ-aminopropylmethyldiethoxysilane in a mass ratio of 1:0.2 to deionized water, stirring mechanically at 300 rpm for 2 hours, centrifuging at 5000 rpm for 30 minutes, washing the centrifuged product with deionized water for 3 times, and vacuum drying at 60° C. for 12 hours to obtain the modified BaSO4 microspheres;

[0047] Step S2, weigh polymethyl methacrylate, mix it with modified BaSO4 microspheres and polyethylene wax evenly, put it into a twin-screw extruder, set the head temperature to 240°C, the screw speed to 200r / min, extrude and granulate, and obtain the light-guiding masterbatch.

[0048] Comparative Example 2

[0049] This comparative example provides a light-guiding masterbatch, comprising the following raw material components in parts by weight: 70 parts of polymethyl methacrylate, 12 parts of PS microspheres and 4 parts of polyethylene wax.

[0050] The above-mentioned light-guiding masterbatch is prepared by the following method:

[0051] Step S1, 0.5g of stabilizer polyvinyl pyrrolidone, 80g of anhydrous ethanol and 20g of deionized water are mixed evenly, mechanically stirred at 300rpm for 30min at room temperature to completely dissolve the polyvinyl pyrrolidone, then the temperature is raised to 60°C, 10g of styrene and 0.1g of initiator 2,2-azobisisobutyronitrile are slowly added dropwise, and then the temperature is raised to 75°C, and the mixture is reacted under nitrogen protection for 18h. After the product is cooled to room temperature, it is centrifuged at 8000rpm in a high-speed centrifuge for 30min, the centrifuged product is washed 3 times with anhydrous ethanol, and vacuum dried at 60°C for 12h to obtain the PS microspheres;

[0052] Step S2, weigh polymethyl methacrylate and dry it at 110° C. for 6 hours, mix it evenly with PS microspheres and polyethylene wax, put it into a twin-screw extruder, set the head temperature to 240° C., the screw speed to 200 r / min, extrude and granulate, and obtain the light-guiding masterbatch.

[0053] Take the light-guiding masterbatch prepared in Example 1-3 and Comparative Example 1-2 and put it into 98% of PMMA by mass at 2% by mass to make injection molding strips. The speed of the injection molding machine is controlled to be 55r / min, and the barrel temperature is: 180°C for the front section, 200°C for the middle section, and 230°C for the rear section; the mold temperature is 80°C, the nozzle temperature is 230°C, the injection pressure is 90MPa, the injection time is controlled to be 8s, the holding time is 15s, and the cooling time is 35s, and a plate-shaped molded product with a thickness of 127×127×3mm is obtained. The dimensional stability, impact strength, light transmittance and haze of the molded product are tested. The test results are shown in Table 1. The test method is as follows:

[0054] (1) The impact strength (unnotched specimen) was tested in accordance with the national standard GB / T 1043.1-2008 “Determination of impact properties of simply supported beams of plastics Part 1”.

[0055] (2) Haze and transmittance: Refer to GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics" to test the light transmittance and haze. With incident light of size 20×1.6mm and diffusion angle 0°, the light transmittance at an optical path length of 115mm and a wavelength of 350nm~800nm ​​is measured.

[0056] (3) Dimensional stability: The molded product was stored at a temperature of 60°C and a relative humidity of 90% for 500 hours, and the dimensional change of the long side before and after storage was measured. Deformation rate = ((long side length after storage) - (long side length before storage)) ÷ (long side length before storage) × 100 (%).

[0057] Table 1

[0058]

[0059]

[0060] The molded products prepared in Examples 1-3 and Comparative Examples 1-2 were placed in the same backlight module and measured using the BM-7 nine-point method. The average brightness values ​​were shown in Table 2.

[0061] Table 2

[0062] <![CDATA[Average luminance cd / m 2 > Uniformity Example 1 7986 96.74% Example 2 7758 95.57% Example 3 7835 96.15% Comparative Example 1 7024 81.83% Comparative Example 2 7133 85.67%

[0063] In summary, the light-guiding masterbatch prepared by the present invention can basically maintain high light efficiency and high uniformity of the product, and the components have good dispersibility and compatibility, are not easy to agglomerate, effectively guarantee the mechanical properties of the product, and have broad application prospects.

[0064] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A light-guiding masterbatch, characterized in that: The method comprises the following raw material components in parts by weight: 60-80 parts of resin base material, 5-15 parts of PS@BaSO4 microspheres and 1-6 parts of dispersant; The PS@BaSO4 microspheres are prepared by using modified BaSO4 microspheres modified by a silane coupling agent as growth sites and by dispersing and polymerizing polystyrene on the surface of the microspheres.

2. The light-guiding masterbatch according to claim 1, characterized in that: The preparation method of the PS@BaSO4 microspheres comprises the following steps: Step S1, adding barium sulfate and a silane coupling agent into deionized water, stirring and reacting for 1-3 hours, centrifuging, washing, and drying to obtain the modified BaSO4 microspheres; Step S2, the modified BaSO4 microspheres, stabilizer polyvinyl pyrrolidone, anhydrous ethanol and deionized water are mixed evenly, styrene and initiator 2,2-azobisisobutyronitrile are added dropwise at 55-65°C, and then the temperature is raised to 70-80°C, and the reaction is carried out under nitrogen protection for 16-24 hours. After the product is cooled to room temperature, it is centrifuged, washed and dried to obtain the PS@BaSO4 microspheres.

3. The light-guiding masterbatch according to claim 2, characterized in that: The silane coupling agent is selected from at least one of 3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane and 3-mercaptopropyltriethoxysilane.

4. The light-guiding masterbatch according to claim 2, characterized in that: In step S1, the mass ratio of the barium sulfate to the silane coupling agent is 1:0.05-0.

3.

5. The light-guiding masterbatch according to claim 2, characterized in that: In step S2, the mass ratio of the modified BaSO4 microspheres, polyvinyl pyrrolidone, styrene, 2,2-azobisisobutyronitrile, anhydrous ethanol and deionized water is 2-4:0.4-0.6:10:0.1:80-90:10-20.

6. The light-guiding masterbatch according to claim 1, characterized in that: The dispersant is selected from at least one of polyacrylamide, polyethylene wax, calcium stearate or hexenyl bisstearamide.

7. The light-guiding masterbatch according to claim 1, characterized in that: The resin substrate is selected from at least one of polycarbonate, polymethyl methacrylate or polystyrene.

8. A method for preparing the light-guiding masterbatch according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: The raw material components are weighed according to the ratio, and the resin substrate, PS@BaSO4 microspheres and dispersant are evenly mixed, and then melt-blended in a twin-screw extruder, extruded and granulated to obtain the light-guiding masterbatch.

9. Use of the light-guiding masterbatch according to any one of claims 1 to 7 in the preparation of light-guiding plates and light-guiding films.

10. The use according to claim 9, wherein the amount of the light-guiding masterbatch added to the light-guiding plate material is 1wt%-20wt%.