Long-carbon-chain binary acid modified interpenetrating network vinyl resin composition and preparation method thereof

By introducing long carbon chain dibasic acid and polyether polyol into the POSS polymerization system, the interpenetrating network structure is formed, and the problem of poor performance of traditional vinyl resins in harsh environments is solved, and high mechanical properties and low smoke and low heat are achieved The released effect is suitable for a variety of application scenarios.

CN118931089APending Publication Date: 2024-11-12HEZE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411132544.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional vinyl resins have poor performance in harsh environments such as high temperature, high humidity, chemical corrosion, etc., and the introduction of POSS rigid molecules may lead to material brittleness and affect practical applications.

Method used

By introducing long carbon chain dibasic acid and polyether polyol into the POSS polymerization system, an interpenetrating network structure is formed, combining the rigidity of POSS and the flexibility of long carbon chain dibasic acid, the complementary component performance is achieved, and a high performance is prepared Interpenetrating network vinyl resin material with mechanical strength, low smoke and low heat release.

Benefits of technology

It achieves high mechanical properties, low smoke and low heat release, good chemical stability and durability of the material, and is suitable for application scenarios that require reduced fire hazards, such as building materials and transportation vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931089A_ABST
    Figure CN118931089A_ABST
Patent Text Reader

Abstract

The invention relates to a long-carbon-chain binary acid modified unsaturated polysilsesquioxane interpenetrating network vinyl resin composition and a preparation method thereof, and belongs to the field of polymeric materials. The preparation method comprises the following steps: firstly, enabling rigid unsaturated polysilsesquioxane to react with a reactive diluent through a polymerization reaction to form a cross-linked network structure; secondly, on the basis of the rigid unsaturated polysilsesquioxane cross-linked network, flexible long-carbon-chain dibasic acid and polyether polyol are introduced, and esterification reaction is carried out; finally, the interpenetrating network polymeric material containing the Si-O-Si structure and the polyester structure at the same time is prepared. The interpenetrating network polymeric material provided by the invention not only shows better mechanical properties, but also has the advantages of low smoke and low heat release during combustion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a long carbon chain dibasic acid modified interpenetrating network vinyl resin composition and a preparation method thereof, in particular to a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin composition and a preparation method thereof, belonging to the field of high molecular polymer materials. Background Art

[0002] As an important polymer material, vinyl resin is widely used in coatings, adhesives, composite materials and other fields due to its good chemical corrosion resistance, electrical properties and processing properties. However, the performance of traditional vinyl resins may not be ideal in certain specific application scenarios, such as high temperature, high humidity, chemical corrosion and other harsh environments. Therefore, modifying vinyl resins to improve their comprehensive performance has become an important direction of current polymer material research. Polyhedral polysilsesquioxane (POSS) has a stable rigid molecular structure with Si-O-Si as the main chain, and the vinyl POSS has good reactivity and thermal stability. However, the introduction of POSS rigid molecules in the polymerization system may also bring brittleness to the material, which is not conducive to the practical application of the material. To solve this problem, it is very necessary to introduce some long-chain flexible molecules into the polymerization system.

[0003] Long carbon chain dibasic acids, such as long carbon chain dibasic acids, polyethylene glycol, and hydroxy-terminated polybutadiene, as compounds with long carbon chains and carboxylic acid groups, have good flexibility and chemical stability. Introducing them into the POSS polymerization system is expected to improve the toughness, chemical corrosion resistance and processing properties of the resin material. At the same time, long carbon chain dibasic acids can also form an interpenetrating network structure with the POSS resin matrix. The complementary combination of a stable cage structure and a flexible long chain structure is expected to produce a polymer material with higher mechanical strength and thermal stability. Summary of the invention

[0004] Based on the above background, the present invention proposes a long carbon chain dibasic acid modified interpenetrating network vinyl resin composition and a preparation method thereof. The method can stably combine polymers with different functions through a specific interpenetrating network technology to achieve performance complementarity between components. The long carbon chain dibasic acid is effectively compounded with the POSS-based vinyl resin to form a resin material with excellent performance. Therefore, combining the advantages of polysilsesquioxane and long carbon chain dibasic acid, this novel interpenetrating network polymer material shows a high research value. The object of the present invention is to provide a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin composition with good mechanical properties, low smoke and low heat release and a preparation method thereof. The method first reacts rigid POSS with a reactive diluent through a polymerization reaction to form a cross-linked network structure. Secondly, on the basis of a rigid POSS cross-linked network, a flexible long carbon chain dibasic acid and a polyether polyol are introduced and a polymerization reaction is carried out. Finally, an interpenetrating network polymer material containing both a POSS structure and a polyester structure is formed. The specific reaction principle is shown in the attached Figure 1 The interpenetrating network polymer material provided by the present invention not only exhibits good mechanical properties, but also has the advantages of low smoke and low heat release during combustion.

[0005] The objectives of the present invention are achieved through the following technical solutions. A long carbon chain dibasic acid modified interpenetrating network vinyl resin composition is prepared from the following components in mass fraction: Long carbon chain dibasic acid 1-45%, preferably 2-30% Unsaturated polysilsesquioxane 10-92%, preferably 20-90% Polyether polyol 1-50%, preferably 2-40% Diluent 3-75%, preferably 3-50% Catalyst 0.05-5%, preferably 0.1-3% Curing agent 0.3-10%, preferably 0.4-8% Accelerator 0.05~6%, preferably 0.1~4%.

[0006] Furthermore, the long carbon chain dibasic acid is a dicarboxylic acid substance with a functionality equal to 2. Preferably, the long carbon chain dibasic acid is a long carbon chain dibasic acid mixed in any proportion with one or more of 11-carbon dibasic acid, 12-carbon dibasic acid, 13-carbon dibasic acid, 14-carbon dibasic acid, 15-carbon dibasic acid, 16-carbon dibasic acid or 18-carbon dibasic acid, and its detailed structure is as follows: .

[0007] Further, the unsaturated polysilsesquioxane refers to one or more of the following formulas A, B, C, D, E, F and G, and the unsaturated polysilsesquioxane refers to a polysilsesquioxane containing vinyl groups and other non-vinyl groups or only vinyl groups around the molecule, and its molecule is composed of an internally stable Si-O-Si structure and its surrounding groups, mainly including cage-shaped unsaturated polysilsesquioxane, random unsaturated polysilsesquioxane and ladder-shaped unsaturated polysilsesquioxane. The detailed structure of the unsaturated polysilsesquioxane is as follows: ; Wherein, R is R1 or R2, R2 is a group without vinyl group, and R in substances A, B, C, D, E, F and G cannot all be R2, and the structures of R1 and X are as follows: .

[0008] Furthermore, the polyether polyol is a polyether polyol substance with a functionality of 2-10, preferably a functionality of 2-6; the polyether polyol is a polyether polyol mixed in any proportion with one or more of polyethylene glycol, polypropylene glycol, polytetrahydrofuran, polytriethanolamine, polyoxypropylene glycol, tetrahydrofuran-oxypropylene copolymer glycol or polyoxytetramethylene glycol.

[0009] Further, the diluent is an unsaturated diluent. Preferably, the diluent is a diluent selected from the group consisting of styrene, acrylic acid, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, methyl methacrylate, ethylene glycol dimethacrylate, methyl acrylate, vinyl acetate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, polyethylene glycol diacrylate, diethylene glycol phthalate diacrylate, propoxylated neopentyl glycol diacrylate, pentaerythritol triacrylate, propoxylated glycerol triacrylate and pentaerythritol tetraacrylate in any proportion. Furthermore, the catalyst is a catalyst selected from one or more of sulfuric acid, phosphoric acid, boric acid, titanate, zirconate, ferric chloride, phosphorus pentoxide, aluminum oxide, sodium hydroxide, sodium carbonate, dicyclohexylcarbodiimide, lipase or acidic resin in any proportion.

[0010] Furthermore, the curing agent is a curing agent selected from the group consisting of methyl ethyl ketone peroxide, cyclohexanone peroxide, benzoyl peroxide, dilauroyl peroxide, acetylacetone peroxide, tert-butyl perbenzoate, and cumene hydroperoxide, mixed in any proportion.

[0011] Furthermore, the accelerator is a mixture of one or more of cobalt isooctanoate, cobalt naphthenate, triethylenediamine, dimethylaniline, sodium dodecylsulfonate, diethylaniline or dimethyl-p-methylaniline in any proportion.

[0012] A long carbon chain dibasic acid modified interpenetrating network vinyl resin composition and a preparation method thereof, wherein the specific preparation steps are as follows: Step 1: stirring, sequentially adding a diluent, a polyether polyol, and a long carbon chain dibasic acid to the unsaturated polysilsesquioxane, and mixing evenly to obtain a stable mixed system; Step 2: Add a catalyst to the mixed system obtained in step 1 and mix well; then add an accelerator, mix well, and then add a curing agent; at this time, continue stirring, and the long-chain polyester structure and the double bond polymerization network structure of the vinyl resin have the conditions for formation and interpenetration, so as to obtain a uniform reaction system; Step 3: thermally cure the reaction system obtained in step 2 until the reaction is complete, thereby obtaining a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material.

[0013] Before step 3 thermal curing, the reaction system obtained in step 2 is evacuated to a vacuum; the vacuum degree of the evacuation reaches -0.01 to -0.09 MPa.

[0014] Furthermore, in step 2, when the catalyst is added and mixed, the mixing temperature is 15 to 90° C. and the mixing time is 1 to 60 min; In step 2, when the accelerator is added and mixed, the mixing temperature is 15 to 80° C. and the mixing time is 1 to 40 min; In step 2, when the curing agent is added and mixed, the mixing temperature is 15 to 70° C. and the mixing time is 1 to 30 min; The thermal curing method in step 3 is: first, cure at a temperature of 20 to 60° C. for 2 to 24 h, then heat to 60 to 80° C. for 1 to 12 h, and finally heat to 80 to 120° C. for 1 to 10 h.

[0015] Beneficial Effects 1) The present invention uses low-smoke, flame-retardant unsaturated polysilsesquioxane as raw material, fully utilizing the rigid molecular structure and internal stable Si-O-Si structure of polysilsesquioxane, which can significantly improve the elastic modulus of the polymer material, and the bending strength is higher than 65 MPa. On the basis of rigid polysilsesquioxane, a flexible polyester structure formed by long carbon chain dibasic acid and polyether polyol is used to reduce the brittleness of the polymer material and ensure good mechanical properties of the material.

[0016] 2) The polymer material produced by the present invention has good comprehensive performance. It has the characteristics of low smoke and good flame retardancy during combustion, with a maximum smoke density lower than 300, an oxygen index higher than 27, and a heat release lower than 65 MJ / m 2 This is mainly due to the synergistic effect of the POSS structure and the modified long-chain dibasic acid, which can inhibit the generation of harmful gases during combustion, reduce smoke and heat release, and improve the safety of the material. This feature has important practical significance for application scenarios that need to reduce fire hazards, such as building materials and transportation.

[0017] 3) The interpenetrating network structure of the present invention gives the material higher chemical stability and durability. The combination of the rigidity of the POSS structure and the flexibility of the long carbon chain dibasic acid can effectively improve the heat resistance, chemical corrosion resistance and aging resistance of the material, ensuring its long-term stable use in harsh environments.

[0018] 4) The interpenetrating network polymer material produced by the present invention contains rich silicon and carbon elements and is halogen-free, has good flame retardant and carbon-forming effects, and is an environmentally friendly polymer material. In addition, the production process is simple, the reaction conditions are mild, the product yield is high, the cost is low, and the technical advantages are obvious.

[0019] In summary, the long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin composition and its preparation method of the present invention achieve excellent mechanical properties, low smoke and low heat release, good processing performance and high stability by optimizing the material structure and modification method, and provide strong technical support for the application of high-performance resin materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention is a reaction principle diagram of a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material. DETAILED DESCRIPTION

[0021] The present invention is further described below in conjunction with specific embodiments, but the scope of protection claimed by the present invention is not limited to the scope involved in the embodiments.

[0022] Example 1 A long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material, the components of which include dodecanedioic acid, cage-shaped unsaturated polysilsesquioxane (A), polyethylene glycol (average molecular weight of 400), hydroxyethyl methacrylate, titanate, benzoyl peroxide and cobalt isooctanoate. The mass fractions of the components are as follows: Dodecanedioic acid 10.0% Cage-shaped unsaturated polysilsesquioxane (A) 48.0% Polyethylene glycol 15.0% Hydroxyethyl Methacrylate 25.0% Titanate 1.0% Benzoyl peroxide 0.6% Cobalt 2-ethylhexanoate 0.4% A method for preparing a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material, the specific preparation steps are: 1) Add 48.0 g of cage-shaped unsaturated polysilsesquioxane (A) and 25.0 g of hydroxyethyl methacrylate into a mixing kettle and stir at 70° C. for 20 min to obtain a first mixed system.

[0023] 2) Add 15.0 g of polyethylene glycol to the first mixed system obtained in 1), and stir the mixture at 70° C. for 30 min to obtain a second mixed system.

[0024] 3) The second mixed system obtained in 2) was maintained at 70° C. 10.0 g of dodecanedioic acid was added and stirred for 20 min to obtain a third mixed system.

[0025] 4) The temperature of the third mixed system obtained in 3) was lowered to 50° C., 1.0 g of titanate was added, and stirred for 5 min to obtain a first reaction system.

[0026] 5) Add 0.4 g of cobalt isooctanoate to the first reaction system obtained in 4), maintain the temperature at 50° C., and continue stirring for 2 minutes to obtain a second reaction system.

[0027] 6) The second reaction system obtained in 5) was cooled to 30°C, and 0.6 g of benzoyl peroxide was added and stirred for 2 minutes to obtain a third reaction system. At this time, the long-chain polyester structure and the double bond polymerization network structure of the vinyl resin have the conditions for formation and interpenetration. 7) Evacuate the third reaction system in 6) and maintain the vacuum for 2 minutes when the vacuum degree reaches about -0.07 MPa.

[0028] 8) The third reaction system obtained in 7) is injected into the mold and placed in an oven for thermal curing. The curing procedure is 30°C for 12 h, 60°C for 10 h, and 100°C for 6 h. Finally, a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material is obtained. Example 2 A long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material, the components of which include hexadecane dibasic acid, unsaturated polysilsesquioxane, polytetrahydrofuran (average molecular weight of 4000), styrene, boric acid, methyl ethyl ketone peroxide and cobalt naphthenate, wherein the unsaturated polysilsesquioxane is a mixture of cage-shaped unsaturated polysilsesquioxane B and random unsaturated polysilsesquioxane D, and the mass ratio is 1:1. The mass fractions of the components are as follows: Hexadecane dibasic acid 8.0% Unsaturated polysilsesquioxane 66.0% Polytetrahydrofuran 10.0% Styrene 14.0% Boric acid 0.5% Methyl ethyl ketone peroxide 1.2% Cobalt naphthenate 0.3% A method for preparing a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material, the specific preparation steps are: 1) Add 66.0 g of unsaturated polysilsesquioxane and 14.0 g of styrene into a mixing kettle and stir at 60° C. for 25 min to obtain a first mixed system.

[0029] 2) Add 10.0 g of polytetrahydrofuran to the first mixed system obtained in 1), maintain stirring at 60° C. for 20 min, and obtain a uniformly mixed second mixed system.

[0030] 3) The second mixed system obtained in 2) was heated to 80° C., 8.0 g of hexadecane dibasic acid was added, and stirred for 10 min to obtain a third mixed system that was uniformly mixed.

[0031] 4) The temperature of the third mixed system obtained in 3) was lowered to 60°C, 0.5 g of boric acid was added, and stirred for 8 min to obtain a first reaction system.

[0032] 5) When the temperature of the first reaction system obtained in 4) is lowered to 30°C, 0.3 g of cobalt cyclohexaneate is added and stirred for 2 min to obtain a second reaction system.

[0033] 6) Add 1.2 g of methyl ethyl ketone peroxide to the second reaction system obtained in 5), maintain the temperature at 30°C and stir for 3 minutes to obtain a third reaction system. At this time, the long-chain polyester structure and the double bond polymerization network structure of the vinyl resin have the conditions for formation and interpenetration. 7) Evacuate the third reaction system in 6) and maintain the vacuum for 2 minutes when the vacuum degree reaches about -0.09 MPa.

[0034] 8) The third reaction system obtained in 7) is injected into a mold and placed in an oven for thermal curing. The curing procedure is 50° C. for 15 h, 80° C. for 6 h, and 110° C. for 3.5 h. Finally, a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material is obtained.

[0035] Example 3 A long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material, the components of which include long carbon chain dibasic acid, unsaturated polysilsesquioxane, polyethylene glycol (average molecular weight of 800), diluent, dicyclohexylcarbodiimide, methyl ethyl ketone peroxide and cobalt naphthenate, wherein the long carbon chain dibasic acid is a mixture of 11 carbon dibasic acid and 16 carbon dibasic acid, and the mass ratio is 2:1; the unsaturated polysilsesquioxane is a mixture of cage-shaped unsaturated polysilsesquioxane B and trapezoidal unsaturated polysilsesquioxane G, and the mass ratio is 1:1; the diluent is a mixture of styrene and ethylene glycol dimethacrylate, and the mass ratio is 1:1. The mass fractions of the components are as follows: Long carbon chain dibasic acid 6.0% Unsaturated polysilsesquioxane 70.0% Polyethylene glycol 6.0 % Diluent 16.0% Dicyclohexylcarbodiimide 1.0% Methyl ethyl ketone peroxide 0.6% Cobalt naphthenate 0.4% A method for preparing a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material, the specific preparation steps are: 1) Add 70.0 g of unsaturated polysilsesquioxane and 17.0 g of diluent into a mixing kettle and stir at 75° C. for 20 min to obtain a first mixed system.

[0036] 2) Add 5.0 g of polyethylene glycol to the first mixed system obtained in 1), and stir at 75° C. for 20 min to obtain a second mixed system.

[0037] 3) The temperature of the second mixed system obtained in 2) was maintained at 75°C, 6.0 g of a long carbon chain dibasic acid was added, and stirred for 10 min to obtain a third mixed system that was uniformly mixed.

[0038] 4) After the temperature of the third mixed system obtained in 3) was lowered to 25° C., 1.0 g of dicyclohexylcarbodiimide was added and stirred for 15 min to obtain a first reaction system.

[0039] 5) Add 0.4 g of cobalt cyclopentaneate to the first reaction system obtained in 4), maintain the temperature at 25° C. and stir for 10 min to obtain a second reaction system. 6) Add 0.6 g of methyl ethyl ketone peroxide to the second reaction system obtained in 5), maintain the temperature at 25°C and stir for 5 minutes to obtain a third reaction system. At this time, the long-chain polyester structure and the double bond polymerization network structure of the vinyl resin have the conditions for formation and interpenetration. 7) Evacuate the third reaction system in 6) and maintain the vacuum for 3 minutes when the vacuum degree reaches about -0.08 MPa.

[0040] 8) The third reaction system obtained in 7) is injected into the mold and placed in an oven for thermal curing. The curing procedure is 60°C for 10 h, 70°C for 6 h, and 100°C for 4 h. Finally, a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material is obtained.

[0041] The compositions prepared in Example 1, Example 2 and Example 3 were poured into a mold according to standard size to prepare test specimens.

[0042] The oxygen index test is carried out in accordance with GB / T 8924 standard, with a sample size of 130 mm × 6.5 mm × 3 mm; the smoke density is tested in accordance with ISO 5659-2 standard, with a radiation cone of 50 kW / m 2 , flameless; heat release test using cone calorimeter, according to ISO 5660 standard, radiant power of 50 kW / m 2 The bending performance test of the resin casting body is carried out in accordance with GB / T 2570-1995 standard, and the sample size is 100 mm× 15 mm× 4 mm.

[0043] The test results of the polymer material properties of each embodiment are shown in Table 1: Table 1. Performance test results of the compositions of various examples The present invention provides a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material and a preparation method thereof. Unsaturated polysilsesquioxane is used as a raw material, and the rigid molecular structure of the polysilsesquioxane is fully utilized to improve the elastic modulus of the polymer material. However, the rigid polysilsesquioxane structure also brings the disadvantage of brittleness to the material. Therefore, in order to solve the problem of material brittleness, a long-chain flexible structure needs to be introduced on the basis of the rigid polysilsesquioxane. The present invention adopts a flexible polyester structure formed by a long carbon chain dibasic acid and a polyether polyol to reduce the brittleness of the polymer material. It can be seen from Table 1 that the interpenetrating network structure combining rigidity and flexibility enables the material to exhibit superior mechanical properties, and the bending strength is above 75MPa. At the same time, the polymer material contains rich silicon and carbon elements, has good flame retardant and carbon-forming effects, and the oxygen index reaches above 26. It exhibits low smoke (maximum smoke density is less than 300) and low heat release (less than 65 MJ / m 2 It can be seen that the long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material provided by the present invention has significant practical application value, and the preparation method is simple and suitable for mass production and application.

[0044] The specific description above further illustrates in detail the purpose, technical solutions and beneficial effects of the invention. It should be understood that the above is only a specific embodiment of the present invention, which is used to explain the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A long carbon chain dibasic acid modified interpenetrating network vinyl resin material, characterized in that: The preparation is obtained by including the following components by mass fraction: Long carbon chain dibasic acid 1~45% Unsaturated polysilsesquioxane 10~92% Polyether polyol 1~50% Diluent 3~75% Catalyst 0.05~5% Curing agent 0.3~10% Accelerator 0.05~6%.

2. The long carbon chain dibasic acid modified interpenetrating network vinyl resin material according to claim 1, characterized in that: The preparation is obtained by including the following components by mass fraction: Long carbon chain dibasic acid 2~30% Unsaturated polysilsesquioxane 20~90% Polyether polyol 2~40% Diluent 3~50% Catalyst 0.1~3% Curing agent 0.4~8% Accelerator 0.1~4%.

3. The material according to claim 1 or 2, characterized in that: The long carbon chain dibasic acid is a dicarboxylic acid substance with a functionality equal to 2, including: one or more of undecane dibasic acid, dodecane dibasic acid, tridecane dibasic acid, tetradecane dibasic acid, pentadecane dibasic acid, hexadecane dibasic acid or octadecane dibasic acid mixed in any proportion, and its detailed structure is as follows: 。 4. The material according to claim 1 or 2, characterized in that: The unsaturated polysilsesquioxane refers to a polysilsesquioxane containing vinyl groups and other non-vinyl groups or only vinyl groups around the molecule, and its molecule is composed of an internally stable Si-O-Si structure and its surrounding groups, mainly including cage-shaped unsaturated polysilsesquioxane, random unsaturated polysilsesquioxane and ladder-shaped unsaturated polysilsesquioxane; the detailed structure of the unsaturated polysilsesquioxane is as follows: ; Wherein, R is R1 or R2, R2 is a group without vinyl group, and R in substances A, B, C, D, E, F and G cannot all be R2, and the structures of R1 and X are as follows: 。 5. The material according to claim 1 or 2, characterized in that: The polyether polyol is a polyether polyol substance with a functionality of 2-10, including: a polyether polyol mixed in any proportion with one or more of polyethylene glycol, polypropylene glycol, polytetrahydrofuran, polytriethanolamine, polyoxypropylene glycol, tetrahydrofuran-oxypropylene copolymer glycol or polyoxytetramethylene glycol.

6. The material according to claim 1 or 2, characterized in that: The diluent is an unsaturated diluent, including: styrene, acrylic acid, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, methyl methacrylate, ethylene glycol dimethacrylate, methyl acrylate, vinyl acetate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, polyethylene glycol diacrylate, diethylene glycol phthalate diacrylate, propoxylated neopentyl glycol diacrylate, pentaerythritol triacrylate, propoxylated glycerol triacrylate or pentaerythritol tetraacrylate, one or more of which are mixed in any proportion.

7. The material according to claim 1 or 2, characterized in that: The catalyst is one or more of sulfuric acid, phosphoric acid, boric acid, titanate, zirconate, ferric chloride, phosphorus pentoxide, aluminum trioxide, sodium hydroxide, sodium carbonate, dicyclohexylcarbodiimide, lipase or acidic resin mixed in any proportion; The curing agent is a curing agent selected from the group consisting of methyl ethyl ketone peroxide, cyclohexanone peroxide, benzoyl peroxide, dilauroyl peroxide, acetylacetone peroxide, tert-butyl perbenzoate, and cumene hydroperoxide, mixed in any proportion; The accelerator is a mixture of one or more of cobalt isooctanoate, cobalt naphthenate, triethylenediamine, dimethylaniline, sodium dodecylsulfonate, diethylaniline or dimethyl-p-methylaniline in any proportion.

8. A method for preparing the material according to claim 1 or 2, characterized in that: The specific preparation steps are: Step 1: stirring, sequentially adding a diluent, a polyether polyol, and a long carbon chain dibasic acid to the unsaturated polysilsesquioxane, and mixing evenly to obtain a stable mixed system; Step 2: Add a catalyst to the mixed system obtained in step 1 and mix well; then add an accelerator, mix well, and then add a curing agent; at this time, continue stirring, and the long-chain polyester structure and the double bond polymerization network structure of the vinyl resin have the conditions for formation and interpenetration, so as to obtain a uniform reaction system; Step 3: thermally cure the reaction system obtained in step 2 until the reaction is complete, thereby obtaining a long carbon chain dibasic acid modified POSS-based interpenetrating network vinyl resin polymer material.

9. The method according to claim 8, characterized in that: Before step 3 thermal curing, the first reaction system obtained in step 2 is subjected to vacuum treatment; the vacuum degree of the vacuum treatment reaches -0.01 to -0.09 MPa; In step 2, when the catalyst is added and mixed, the mixing temperature is 15 to 90° C. and the mixing time is 1 to 60 min; In step 2, when the accelerator is added and mixed, the mixing temperature is 15 to 80° C. and the mixing time is 1 to 40 min; In step 2, when the curing agent is added and mixed, the mixing temperature is 15 to 70° C. and the mixing time is 1 to 30 min; The thermal curing method in step 3 is: first, cure at a temperature of 20 to 60° C. for 2 to 24 h, then heat to 60 to 80° C. for 1 to 12 h, and finally heat to 80 to 120° C. for 1 to 10 h.