ABS (Acrylonitrile Butadiene Styrene) resin composition for automobile spoiler and preparation method of ABS resin composition
By adding special admixtures to the ABS resin composition, the problem of the decline in mechanical properties of ABS/PC plastic after adding conductive carbon black is solved, the antistatic properties and mechanical properties are improved, and the electrostatic charge leakage of automobile spoilers is achieved and neutralize.
Patent Information
- Application Number
- CN202411200899.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ABS/PC plastics have caused the mechanical properties of the material to decline after adding conductive carbon black as an antistatic agent.
By adding a special admixture to the ABS resin composition, the admixture prepared by raw materials such as 1,3,5-triaminobenzene, para-cyanobenzaldehyde, para-phenylenediamine, etc., combine amino groups and hydrophobic groups to form conductive The layer is used to reduce the surface resistivity of the material and prepare the ABS resin composition through a twin screw extrusion mechanism.
It improves the antistatic properties, mechanical properties and durability of the material, improves the strength and aging resistance of the material, and realizes the electrostatic charge leakage and neutralization of the automotive spoiler.
Smart Images

Figure BDA0005017814590000071 
Figure BDA0005017814590000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic materials, and in particular to an ABS resin composition for an automobile spoiler and a preparation method thereof. Background Art
[0002] With the development of the automobile industry and the continuous expansion of automobile scale and improvement of performance, the development of parts and related materials industries has been driven. At present, the main direction of the development of automobile material technology in the world is lightweight and environmentally friendly. Reducing the weight of the car itself is one of the most effective measures to reduce automobile emissions and improve combustion efficiency. In order to reduce the cost and weight of the whole vehicle and increase the effective load of the car, plastics are increasingly widely used in the automobile industry. Automobile plastic parts are divided into three categories: interior parts, exterior parts and functional parts.
[0003] Acrylonitrile-butadiene-styrene (ABS) is a widely used engineering plastic. The acrylonitrile in ABS gives ABS good heat resistance, chemical resistance and tensile strength; butadiene gives good toughness and impact resistance; styrene gives good gloss, rigidity and easy processing. Usually, the proportion of each component is generally 10-30% butadiene, 10-30% acrylonitrile, and 30-60% styrene. The overall performance can be changed by adjusting the proportion of the three components. For example, increasing the proportion of polystyrene can improve the flow properties of, and controlling the proportion of acrylonitrile at 25-27% is conducive to improving the compatibility with; increasing the proportion of butadiene can improve the toughness of. The above characteristics make ABS have the following characteristics: excellent room temperature and low temperature toughness, good processing fluidity, excellent chemical resistance, good colorability, high gloss and good water resistance, so that it has been widely used in electronic appliances, instruments and meters, automotive parts, building materials and other fields. However, ABS has insufficient mechanical properties. ABS is mixed with polycarbonate (PC) to form an alloy. ABS / PC plastic is a polymer alloy commonly used in industry, in which PC improves the alloy's good heat resistance and excellent dimensional stability. ABS reduces the cost of materials while providing good processing fluidity. It effectively improves the mechanical and heat resistance of ABS. However, ABS / PC plastic is prone to static electricity during transportation or use, resulting in undesirable phenomena such as dust absorption, electric shock, and even spark discharge. The current common method for preparing antistatic polymers is to add antistatic agents to polymers. In the prior art, the commonly used antistatic agent is conductive carbon black. Directly adding conductive carbon black causes the mechanical properties of ABS / PC plastics to decrease. Summary of the invention
[0004] The object of the present invention is to provide an ABS resin composition for automobile spoiler and a preparation method thereof, so as to solve the following technical problems:
[0005] Adding conductive carbon black as an antistatic agent to existing ABS / PC plastics leads to a decrease in the mechanical properties of the material.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing an ABS resin composition for an automobile spoiler comprises the following steps:
[0008] Premixing ABS high-rubber powder, polycarbonate, auxiliary agents and additives in a high-speed mixer to obtain a premix; melting and extruding the premix through a twin-screw extruder, cooling and granulating, to obtain an ABS resin composition;
[0009] The preparation method of the admixture comprises the following steps:
[0010] S1: In a nitrogen atmosphere, 1,3,5-triaminobenzene, p-cyanobenzaldehyde, 1,2-dichlorobenzene and cesium carbonate are placed in a reaction bottle, the temperature is controlled at 140-160°C, the reaction is kept warm for 60-84 hours, air is introduced, mechanical stirring is performed, the mixture is filtered, washed and dried, and calcined in a muffle furnace to obtain component 1;
[0011] S2: Put component 1, p-phenylenediamine and methanol in a reaction kettle, control the temperature at 15-25°C, keep the reaction for 0.5-1h, wash and dry to obtain component 2;
[0012] S3: Add component 2, isopropanol and deionized water into a reaction kettle, stir evenly mechanically, add aniline salt solution, stir evenly mechanically, add ammonium persulfate, cool to 0-5°C, react while stirring, wash and dry to obtain an admixture.
[0013] As a further embodiment of the present invention: the mass ratio of 1,3,5-triaminobenzene, p-cyanobenzaldehyde, 1,2-dichlorobenzene and cesium carbonate in S1 is 100:20-40:1500-6500:0.1-10.
[0014] As a further solution of the present invention: the mass ratio of component 1, p-phenylenediamine and methanol in S2 is 100:30-60:700-2100.
[0015] As a further solution of the present invention: the mass ratio of component 2, isopropanol, deionized water, aniline salt solution and ammonium persulfate in S3 is 100:350-500:2000-3500:3000-5000:50-80.
[0016] As a further solution of the present invention: the additive accounts for 10-15% of the total mass of the ABS resin composition.
[0017] As a further solution of the present invention: the weight average molecular weight of ABS high-rubber powder is 1×105 -5×10 5 g / mol, polybutadiene content>40%, ABS high-rubber powder melt flow rate at 300℃×1.2kg is 1-10g / 10min; ABS high-rubber powder accounts for 20-50% of the total mass of the ABS resin composition.
[0018] As a further solution of the present invention: the melt flow rate of the polycarbonate is 1-10 g / 10 min at 300° C.×1.2 kg, and the polycarbonate accounts for 40-60% of the total mass of the ABS resin composition.
[0019] As a further embodiment of the present invention: the auxiliary agent includes an antioxidant, a release agent, and a UV absorber;
[0020] The antioxidant is any one of a hindered phenol antioxidant and a phosphite antioxidant or a mixture of several of them in any ratio; the antioxidant accounts for 0.4-1% of the total mass of the ABS resin composition;
[0021] The mold release agent is a silicone mold release agent; the mold release agent accounts for 0.4-1% of the total mass of the ABS resin composition;
[0022] The ultraviolet absorber is any one of benzophenone ultraviolet absorbers, benzotriazole ultraviolet absorbers and piperidine ultraviolet absorbers or a mixture of several of them in any ratio; the ultraviolet absorber accounts for 0.3-2% of the total mass of the ABS resin composition.
[0023] As a further solution of the present invention: the extrusion temperature of the twin-screw extruder is: 220-250°C; the extrusion speed is 200-450rpm.
[0024] An ABS resin composition for automobile spoilers is prepared by any one of the above preparation methods.
[0025] Beneficial effects of the present invention:
[0026] (1) The present invention uses 1,3,5-triaminobenzene and p-cyanobenzaldehyde as raw materials, and obtains component one through Knoevenage l reaction polycondensation, and component one has a large number of cyano groups; the present invention continues to use component one and p-phenylenediamine as raw materials, and utilizes the cyano groups on component one to react with the amino groups on p-phenylenediamine to obtain component two. Finally, component two and aniline are used as raw materials to react and prepare an additive. The present invention adds an additive to the ABS resin composition to give the ABS resin composition excellent antistatic properties.
[0027] (2) The hydrophobic group of the additive prepared by the present invention is combined with the ABS resin composition, and the hydrophilic groups such as amino groups adsorb the monomolecular conductive layer of trace moisture in the air, which reduces the surface resistivity of the material and accelerates the leakage of static charge. The combination of the additive and the organic matter in the ABS resin composition not only improves the strength and aging resistance of the material, but also improves the mechanical properties and durability of the material; and a large conjugated system is formed inside the additive, which is conducive to the flow of electrons, forming a conductive three-dimensional network to transfer charge carriers by relying on the direct contact of particles in the chain organization, thereby realizing the leakage and neutralization of the static charge of the automobile spoiler. DETAILED DESCRIPTION
[0028] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The preparation method of the admixture of embodiment 1 comprises the following steps:
[0030] S1: 10 g of 1,3,5-triaminobenzene and 2.4 mL of p-cyanobenzaldehyde were subjected to three freeze-thaw cycles respectively and then added to a reaction bottle in sequence, 155 mL of 1,2-dichlorobenzene and 0.05 g of cesium carbonate were added to the reaction bottle, the temperature was raised to 145°C in a nitrogen atmosphere, the reaction was kept warm for 66 hours, air was introduced, mechanical stirring was performed, the mixture was filtered, washed with water and tetrahydrofuran in sequence, vacuum dried, and calcined in a muffle furnace to obtain component 1;
[0031] S2: 5 g of component 1, 1.5 g of p-phenylenediamine and 52.5 mL of methanol were placed in a reaction kettle, the temperature was controlled at 15°C, the reaction was kept warm for 0.5 h, and then washed with water and dried to obtain component 2;
[0032] S3: Add 5g of component 2, 22.5mL of isopropanol and 100mL of deionized water into a reactor, stir evenly mechanically, add 175g of aniline salt solution, stir evenly mechanically, add 2.5g of ammonium persulfate, cool to 0°C, keep warm while stirring, wash with 0.1mol / L hydrochloric acid, anhydrous ethanol and distilled water in turn, and dry in vacuo to obtain an admixture.
[0033] The aniline salt solution is prepared by adding 1 g of aniline into 100 mL of a 2.5 mol / L hydrochloric acid aqueous solution.
[0034] The preparation method of the admixture of embodiment 2 comprises the following steps:
[0035] S1: 10 g of 1,3,5-triaminobenzene and 3 mL of p-cyanobenzaldehyde were subjected to three freeze-thaw cycles respectively and then added to a reaction bottle in sequence, 300 mL of 1,2-dichlorobenzene and 0.5 g of cesium carbonate were added to the reaction bottle, the temperature was raised to 150°C in a nitrogen atmosphere, the reaction was kept warm for 72 hours, air was introduced, mechanical stirring was performed, the mixture was filtered, washed with water and tetrahydrofuran in sequence, vacuum dried, and calcined in a muffle furnace to obtain component 1;
[0036] S2: 5 g of component 1, 2.2 g of p-phenylenediamine and 90 mL of methanol were placed in a reaction kettle, the temperature was controlled at 20°C, the reaction was kept warm for 0.8 h, and then washed with water and dried to obtain component 2;
[0037] S3: Add 5g of component 2, 27.5mL of isopropanol and 150mL of deionized water into a reactor, stir evenly mechanically, add 200g of aniline salt solution, stir evenly mechanically, add 3.2g of ammonium persulfate, cool to 2°C, keep warm while stirring, wash with 0.1mol / L hydrochloric acid, anhydrous ethanol and distilled water in turn, and dry in vacuo to obtain an admixture.
[0038] The aniline salt solution is prepared by adding 1 g of aniline into 100 mL of a 2.5 mol / L hydrochloric acid aqueous solution.
[0039] The preparation method of the additive of embodiment 3 comprises the following steps:
[0040] S1: 10 g of 1,3,5-triaminobenzene and 3.3 mL of p-cyanobenzaldehyde were subjected to three freeze-thaw cycles respectively and then added to a reaction bottle in sequence, 450 mL of 1,2-dichlorobenzene and 1 g of cesium carbonate were added to the reaction bottle, the temperature was raised to 155°C in a nitrogen atmosphere, the reaction was kept warm for 78 h, air was introduced, mechanical stirring was performed, the mixture was filtered, washed with water and tetrahydrofuran in sequence, vacuum dried, and calcined in a muffle furnace to obtain component 1;
[0041] S2: 5 g of component 1, 3 g of p-phenylenediamine and 125 mL of methanol were placed in a reaction kettle, the temperature was controlled at 25°C, the reaction was kept warm for 1 hour, and then washed with water and dried to obtain component 2;
[0042] S3: Add 5g of component 2, 31.5mL of isopropanol and 175mL of deionized water into a reactor, stir evenly mechanically, add 225g of aniline salt solution, stir evenly mechanically, add 4g of ammonium persulfate, cool to 5°C, keep warm while stirring, wash with 0.1mol / L hydrochloric acid, anhydrous ethanol and distilled water in turn, and dry in vacuum to obtain conductive porous carbon.
[0043] The aniline salt solution is prepared by adding 1 g of aniline into 100 mL of a 2.5 mol / L hydrochloric acid aqueous solution.
[0044] Example 4 A method for preparing an ABS resin composition for a car spoiler comprises the following steps: 47 g of ABS high-rubber powder (weight average relative molecular mass is 1×10 5 -5×10 5 g / mol, polybutadiene content>40%, ABS high rubber powder melt flow rate at 300°C×1.2kg is 1-10g / 10min), 40g polycarbonate (melt flow rate at 300°C×1.2kg is 1-10g / 10min), 0.5g 2,6-di-tert-butyl-4-methylphenol), 0.5g tris(2,4-di-tert-butylphenyl)phosphite, 0.6g silicone powder K6105, 1.4g 2-hydroxy-4-octyloxybenzophenone, and 10g of the additive prepared in Example 1 are premixed in a high-speed mixer to obtain a premix; the premix is melt-extruded through a twin-screw extruder (extrusion temperature: 220-250°C; extrusion speed: 200-450rpm), cooled and granulated to obtain an ABS resin composition.
[0045] Example 5 A method for preparing an ABS resin composition for a car spoiler comprises the following steps: 47 g of ABS high-rubber powder (weight average relative molecular mass is 1×10 5 -5×10 5 g / mol, polybutadiene content>40%, ABS high rubber powder melt flow rate at 300°C×1.2kg is 1-10g / 10min), 40g polycarbonate (melt flow rate at 300°C×1.2kg is 1-10g / 10min), 0.5g 2,6-di-tert-butyl-4-methylphenol), 0.5g tris(2,4-di-tert-butylphenyl)phosphite, 0.6g silicone powder K6105, 1.4g 2-hydroxy-4-octyloxybenzophenone, and 10g of the additive prepared in Example 2 are premixed in a high-speed mixer to obtain a premix; the premix is melt-extruded through a twin-screw extruder (extrusion temperature: 220-250°C; extrusion speed: 200-450rpm), cooled and granulated to obtain an ABS resin composition.
[0046] Example 6 A method for preparing an ABS resin composition for a car spoiler comprises the following steps: 47 g of ABS high-rubber powder (weight average relative molecular mass is 1×10 5 -5×10 5g / mol, polybutadiene content>40%, ABS high rubber powder melt flow rate at 300°C×1.2kg is 1-10g / 10min), 40g polycarbonate (melt flow rate at 300°C×1.2kg is 1-10g / 10min), 0.5g 2,6-di-tert-butyl-4-methylphenol), 0.5g tris(2,4-di-tert-butylphenyl)phosphite, 0.6g silicone powder K6105, 1.4g 2-hydroxy-4-octyloxybenzophenone, and 10g of the additive prepared in Example 3 are premixed in a high-speed mixer to obtain a premix; the premix is melt-extruded through a twin-screw extruder (extrusion temperature: 220-250°C; extrusion speed: 200-450rpm), cooled and granulated to obtain an ABS resin composition.
[0047] Comparative Example 1 Compared with Example 4, Comparative Example 1 only replaces the additive added in Example 4 with conductive carbon black in equal amount, and the other components and preparation method are completely consistent with Example 4.
[0048] Performance Testing
[0049] (1) Notched impact strength: tested according to ASTM D256, using an impact tester from Ray-Ran, UK. The specimen size was 64 mm × 12.7 mm × 3.2 mm, and the notch depth was 2.2 mm. The test results are shown in Table 1.
[0050] (2) Tensile properties: The test was conducted according to ASTM D638, using an Instron 4456 electronic tensile testing machine from Instron, UK. The sample size was 168 mm × 13 mm × 3.2 mm, and the test speed was 50 mm / min. The test results are shown in Table 1.
[0051] (3) Bending properties: The test was conducted according to ASTM D790 using an Instron 4456 electronic tensile testing machine from Instron, UK. The specimen size was 64 mm × 12.7 mm × 3.2 mm, the span was 50 mm, and the test speed was 3 mm / min. The test results are shown in Table 1.
[0052] (4) Electrical properties: According to GB / T 1410-2006, the sample size is 100 mm × 100 mm × 100 mm, and it is placed at 23°C and 50% humidity for 24 h before testing. The test results are shown in Table 1;
[0053] Table 1: Statistical table of performance test data of Examples 4-6 and Comparative Example 1
[0054]
[0055]
[0056] It can be seen from Table 1 that the additive prepared in the present application is added to the ABS composition, which not only gives the material good antistatic properties, but also effectively improves the mechanical properties of the material.
[0057] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for preparing an ABS resin composition for an automobile spoiler, characterized in that: The steps include: Premixing ABS high-glue, polycarbonate, auxiliary agent and additive in a high-speed mixer to obtain a premix; melting and extruding the premix through a twin-screw extruder, cooling and granulating to obtain an ABS resin composition; The preparation method of the admixture comprises the following steps: S1: In a nitrogen atmosphere, 1,3,5-triaminobenzene, p-cyanobenzaldehyde, 1,2-dichlorobenzene and cesium carbonate are placed in a reaction bottle, the temperature is controlled at 140-160°C, the reaction is kept warm for 60-84 hours, air is introduced, mechanical stirring is performed, the mixture is filtered, washed and dried, and calcined in a muffle furnace to obtain component 1; S2: Put component 1, p-phenylenediamine and methanol in a reaction kettle, control the temperature at 15-25°C, keep the reaction for 0.5-1h, wash and dry to obtain component 2; S3: Add component 2, isopropanol and deionized water into a reaction kettle, stir evenly mechanically, add aniline salt solution, stir evenly mechanically, add ammonium persulfate, cool to 0-5°C, react while stirring, wash and dry to obtain an admixture.
2. The method for preparing an ABS resin composition for a vehicle spoiler according to claim 1, characterized in that: The mass ratio of 1,3,5-triaminobenzene, p-cyanobenzaldehyde, 1,2-dichlorobenzene and cesium carbonate in S1 is 100:20-40:1500-6500:0.1-10.
3. The method for preparing an ABS resin composition for a vehicle spoiler according to claim 1, characterized in that: The mass ratio of component 1, p-phenylenediamine and methanol in S2 is 100:30-60:700-2100.
4. The method for preparing an ABS resin composition for a vehicle spoiler according to claim 1, characterized in that: The mass ratio of component 2, isopropanol, deionized water, aniline salt solution and ammonium persulfate in S3 is 100:350-500:2000-3500:3000-5000:50-80.
5. The method for preparing an ABS resin composition for a vehicle spoiler according to claim 1, characterized in that: The additive accounts for 10-15% of the total mass of the ABS resin composition.
6. The method for preparing an ABS resin composition for a vehicle spoiler according to claim 1, characterized in that: The weight average molecular weight of the ABS high-rubber powder is 1×10 5 -5×10 5 g / mol, polybutadiene content>40%, ABS high-rubber powder melt flow rate at 300℃×1.2kg is 1-10g / 10min; ABS high-rubber powder accounts for 20-50% of the total mass of the ABS resin composition.
7. The method for preparing an ABS resin composition for a vehicle spoiler according to claim 1, characterized in that: The polycarbonate melt flow rate is 1-10 g / 10 min under the condition of 300° C.×1.2 kg, and the polycarbonate accounts for 40-60% of the total mass of the ABS resin composition.
8. The method for preparing an ABS resin composition for a vehicle spoiler according to claim 1, characterized in that: The auxiliary agents include antioxidants, release agents, and ultraviolet absorbers; The antioxidant is any one of a hindered phenol antioxidant and a phosphite antioxidant or a mixture of several of them in any ratio; the antioxidant accounts for 0.4-1% of the total mass of the ABS resin composition; The mold release agent is a silicone mold release agent; the mold release agent accounts for 0.4-1% of the total mass of the ABS resin composition; The ultraviolet absorber is any one of benzophenone ultraviolet absorbers, benzotriazole ultraviolet absorbers and piperidine ultraviolet absorbers or a mixture of several of them in any ratio; the ultraviolet absorber accounts for 0.3-2% of the total mass of the ABS resin composition.
9. The method for preparing an ABS resin composition for a vehicle spoiler according to claim 1, characterized in that: The extrusion temperature of the twin-screw extruder is 220-250°C; the extrusion speed is 200-450rpm.
10. An ABS resin composition for a car spoiler, characterized in that: Prepared by the preparation method described in any one of claims 1 to 9.