Bio-based toughened flame-retardant PLA / ABS composite material and preparation method thereof

By combining modified polydimethylsiloxane with caprolactone additive and nucleating agent, the compatibility and flame retardant properties of PLA/ABS composite materials are improved, and the flexibility and heat resistance of PLA resin are solved. and the problem of flame retardancy, the effect of bio-based toughening and flame retardant is achieved.

CN118931135AActive Publication Date: 2024-11-12SHENZHEN FUHENG PLASTICS PIGMENT
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411233145.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

PLA resin has insufficient flexibility, low impact strength, low thermal deformation temperature and poor heat resistance, and poor compatibility with ABS resin, making it difficult to obtain flame retardant composite materials.

Method used

Modified polydimethylsiloxane and caprolactone as additives are used to make it through ring-opening polymerization reaction, combined with nucleating agents, improve the compatibility and flame retardant properties of PLA/ABS composite materials, and use siloxanes Thermal flame retardant effect of flexible chains and polycaprolactone chain ends enhances the mechanical and weathering properties of the composite material.

Benefits of technology

The flexibility, impact strength, thermal stability and flame retardant properties of PLA/ABS composite materials are significantly improved, and the poor heat resistance and compatibility problems of PLA resin are solved, thus achieving the effect of bio-based toughening and flame retardant.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a bio-based toughened flame-retardant PLA / ABS composite material and a preparation method thereof, and belongs to the technical field of preparation of PLA composite materials. The material comprises the following raw materials in parts by weight: 75-90 parts of PLA resin, 10-25 parts of ABS resin, 10-20 parts of an auxiliary agent and 0.5-1.5 parts of a nucleating agent, the auxiliary agent is prepared by carrying out ring-opening polymerization reaction on modified polydimethylsiloxane and caprolactone under the action of a ring-opening catalyst; the modified polydimethylsiloxane is prepared by reacting diamino propyl polydimethylsiloxane with a reaction type weather-resistant compound. According to the invention, the assistant is introduced, a siloxane flexible chain end and a polycaprolactone chain end in a molecular structure of the assistant are utilized, the assistant is used as a compatilizer and has heat-resistant and flame-retardant effects, and the toughness of the obtained composite material is improved through the cooperation of the assistant, the ABS resin and the nucleating agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PLA composite material preparation, and specifically relates to a bio-based toughened flame-retardant PLA / ABS composite material and a preparation method thereof. Background Art

[0002] PLA resin refers to polylactic acid resin, also known as polylactide, which is a polyester polymer obtained by polymerization with lactic acid as the main raw material. It has good biodegradability, mechanical properties, and transparent appearance. However, PLA also has some disadvantages, such as insufficient flexibility, low impact strength, low heat deformation temperature, and poor heat resistance. These disadvantages limit the application field of PLA. ABS resin refers to acrylonitrile-styrene-butadiene copolymer, in which ABS is the acronym of Acrylonitrile Butadiene Styrene. It has good impact strength, dimensional stability, dyeability, mechanical strength, rigidity and corrosion resistance, as well as low water absorption, and also has very good transparency and polishing effect. It is the preferred material to replace PC sheet. Therefore, introducing ABS into PLA resin to make alloy resin can effectively improve the shortcomings of insufficient flexibility, low impact strength, low heat deformation temperature, and poor heat resistance of PLA resin. However, the compatibility of PLA and ABS is poor, and it is impossible to fully obtain flame-retardant PLA composite materials by simply relying on the filling of ABS.

[0003] Based on this, the present invention provides a bio-based toughened flame-retardant PLA / ABS composite material and a preparation method thereof. Summary of the invention

[0004] In view of the problem provided in the technical background, the present invention provides a bio-based toughened flame-retardant PLA / ABS composite material and a preparation method thereof.

[0005] One object of the present invention can be achieved by the following technical solutions:

[0006] A bio-based toughened flame-retardant PLA / ABS composite material, comprising the following raw materials in parts by weight: 75-90 parts of PLA resin, 10-25 parts of ABS resin, 10-20 parts of auxiliary agent, and 0.5-1.5 parts of nucleating agent;

[0007] The auxiliary agent is prepared by a ring-opening polymerization reaction of modified polydimethylsiloxane and caprolactone under the action of a ring-opening catalyst;

[0008] The modified polydimethylsiloxane is prepared by reacting bisaminopropyl polydimethylsiloxane with a reactive weather-resistant compound.

[0009] Furthermore, the reaction conditions of the ring-opening polymerization reaction are: a reaction temperature of 90-130° C. and a reaction time of 12-48 hours under a nitrogen atmosphere.

[0010] Furthermore, the mass ratio of the modified polydimethylsiloxane to caprolactone is 15-25:5-8.

[0011] Furthermore, the ring-opening catalyst is one of stannous isooctanoate, dibutyltin dilaurate, trifluoromethanesulfonic acid, and hydrofluoric acid.

[0012] Preferably, the reaction for obtaining the auxiliary agent comprises the following steps:

[0013] After the modified polydimethylsiloxane and caprolactone are mixed, a ring-opening catalyst is added under nitrogen atmosphere at 90-130°C with stirring, and the reaction is continued with heat preservation and stirring for 12-48 hours. The reaction is stopped, and the product is repeatedly treated (dispersed, precipitated, washed, centrifuged) with a dichloromethane and isopropanol system, and finally dried to obtain an auxiliary agent.

[0014] Furthermore, the reaction conditions for obtaining the modified polydimethylsiloxane are: reaction temperature of 0-20° C., and reaction time of 3-8 h.

[0015] Furthermore, the mass ratio of the bisaminopropyl polydimethylsiloxane to the reactive weather-resistant compound is 15-25:3.

[0016] Further, the number average molecular weight of the bisaminopropyl polydimethylsiloxane is 1000-2000;

[0017] Preferably, the number average molecular weight of the bisaminopropyl polydimethylsiloxane is 1000-1500 or 1500-2000.

[0018] Preferably, the reaction for obtaining the modified polydimethylsiloxane comprises the following steps:

[0019] Mix bisaminopropyl polydimethylsiloxane, reactive weather-resistant compound, triethylamine and dichloromethane at 0-5°C, slowly heat to room temperature (20±5°C), stir to react for 3-8h, stop the reaction, rotary evaporate, wash with water, centrifuge, and dry to obtain modified polydimethylsiloxane.

[0020] Furthermore, the reactive weather-resistant compound is prepared by reacting chloroacetyl chloride and 2,4-dihydroxybenzophenone in the presence of an organic solvent and an acid-binding agent at 0-25°C.

[0021] Furthermore, the molar ratio of chloroacetyl chloride to 2,4-dihydroxybenzophenone is 1.1-1.3:1.

[0022] Furthermore, the organic solvent is one of dichloromethane, polytetrahydrofuran, N,N-dimethylformamide and xylene.

[0023] Preferably, the acidifying agent is triethylamine.

[0024] Furthermore, the nucleating agent is a mixture of an organic nucleating agent and an inorganic nucleating agent in a mass ratio of 2-3:1.

[0025] Further, the organic nucleating agent is one of TMC-328 and TMC-300 or a mixture of the two in any ratio;

[0026] Preferably, the organic nucleating agent is TMC-300.

[0027] Furthermore, the inorganic nucleating agent is one of carbon nanotubes, zinc oxide whiskers, and calcium carbonate whiskers;

[0028] Preferably, the inorganic nucleating agent is carbon nanotubes.

[0029] Another object of the present invention can be achieved by the following technical solutions:

[0030] A method for preparing a bio-based toughened flame-retardant PLA / ABS composite material, comprising:

[0031] The PLA resin, ABS resin, auxiliary agent and nucleating agent are mixed, melt-blended, extruded and granulated to obtain a composite material.

[0032] Furthermore, the temperature during the melt blending extrusion is 200-240° C., and the rotation speed is 200-400 r / min.

[0033] Beneficial effects of the present invention:

[0034] The invention discloses a bio-based toughened flame-retardant PLA / ABS composite material and a preparation method thereof. By introducing an auxiliary agent, the siloxane flexible chain end and the polycaprolactone chain end in the auxiliary agent molecular structure are utilized to exert the auxiliary agent as a compatibilizer and heat-resistant flame-retardant effect. The polycaprolactone chain end and the PLA resin chain segment are both polyester-type chain segments and have good compatibility with the PLA resin chain segment. The siloxane flexible chain can be compatible with the ABS resin molecular chain segment, so that the auxiliary agent acts as a compatibilizer, and the PLA resin and the ABS resin have good mixing processability. The siloxane flexible chain plays the role of a silicon-based flame retardant during combustion, and improves the flame retardant property of the composite material. Furthermore, the auxiliary agent molecular chain also contains a benzophenone light-absorbing structure, so that the problem of low weatherability of the composite material due to the introduction of the ABS resin is solved, and the weatherability of the obtained composite material is improved. Finally, the nucleating agent promotes the crystallization property of the PLA resin, and cooperates with the auxiliary agent and the ABS resin to solve the problem of insufficient flexibility of the PLA resin. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] Preparation of additives:

[0038] Preparation of reactive weather-resistant compound: 0.1 mol 2,4-dihydroxybenzophenone, 0.12 mol triethylamine and 60 mL dichloromethane were mixed evenly, and then 0.12 mol chloroacetyl chloride was added dropwise at 0-3°C. After the addition was complete, the temperature was slowly raised to room temperature, and the reaction was continued with stirring for 4 hours. The reaction was stopped, cooled, washed with water, separated, and the organic phase was recrystallized with methanol and dried to obtain a reactive weather-resistant compound;

[0039] Preparation of modified polydimethylsiloxane: 15g of bisaminopropyl polydimethylsiloxane, 3g of reactive weather-resistant compound, 1.5g of triethylamine and 100mL of dichloromethane were mixed uniformly at 0-5°C, slowly heated to room temperature (20±5°C), stirred for reaction for 3h, the reaction was stopped, rotary evaporated, washed with water, centrifuged, and dried to obtain modified polydimethylsiloxane; wherein the number average molecular weight of bisaminopropyl polydimethylsiloxane is 1000-1500;

[0040] Preparation of the auxiliary agent: 15 g of modified polydimethylsiloxane and 5 g of caprolactone were mixed, and then 0.4 g of stannous isooctanoate was added under nitrogen atmosphere, 90 ° C, and the reaction was continued with insulation and stirring for 24 hours. The reaction was stopped, and the product was repeatedly treated with dichloromethane and isopropanol system (dispersion, precipitation, washing, centrifugation), and finally dried to obtain the auxiliary agent.

[0041] Example 2

[0042] Preparation of additives:

[0043] Preparation of reactive weather-resistant compound: 0.1 mol 2,4-dihydroxybenzophenone, 0.13 mol triethylamine and 60 mL dichloromethane were mixed evenly, and then 0.13 mol chloroacetyl chloride was added dropwise at 0-3°C. After the addition was complete, the temperature was slowly raised to room temperature, and the reaction was continued with stirring for 6 hours. The reaction was stopped, cooled, washed with water, separated, and the organic phase was recrystallized with methanol and dried to obtain a reactive weather-resistant compound;

[0044] Preparation of modified polydimethylsiloxane: 25g of bisaminopropyl polydimethylsiloxane, 3g of reactive weather-resistant compound, 1.5g of triethylamine and 100mL of dichloromethane were mixed uniformly at 0-5°C, slowly heated to room temperature (20±5°C), stirred for reaction for 8h, the reaction was stopped, rotary evaporated, washed with water, centrifuged, and dried to obtain modified polydimethylsiloxane; wherein the number average molecular weight of bisaminopropyl polydimethylsiloxane is 1500-2000;

[0045] Preparation of the auxiliary agent: 25 g of modified polydimethylsiloxane and 8 g of caprolactone were mixed, and then 0.63 g of stannous isooctanoate was added under nitrogen atmosphere, 90-130 ° C, and the reaction was continued with insulation and stirring for 48 hours. The reaction was stopped, and the product was repeatedly treated with dichloromethane and isopropanol system (dispersion, precipitation, washing, centrifugation), and finally dried to obtain the auxiliary agent.

[0046] Example 3

[0047] Preparation of PLA / ABS composites:

[0048] Prepare the following raw materials in parts by weight: 75 parts of PLA resin, 25 parts of ABS resin, 20 parts of the auxiliary agent prepared in Example 1, and 0.5 parts of a nucleating agent; wherein the nucleating agent is a mixture of TMC-300 and carbon nanotubes in a mass ratio of 2:1;

[0049] Melt extrusion: PLA resin, ABS resin, additives and nucleating agents are mixed, melt blended and extruded, and granulated to obtain a composite material, wherein the temperature during the melt blending and extrusion is 200-240°C and the rotation speed is 200-400r / min.

[0050] Example 4

[0051] Preparation of PLA / ABS composites:

[0052] Prepare the following raw materials in parts by weight: 85 parts of PLA resin, 15 parts of ABS resin, 15 parts of the auxiliary agent prepared in Example 2, and 1 part of a nucleating agent; the nucleating agent is a mixture of TMC-300 and carbon nanotubes in a mass ratio of 2.5:1;

[0053] Melt extrusion: PLA resin, ABS resin, additives and nucleating agents are mixed, melt blended and extruded, and granulated to obtain a composite material, wherein the temperature during the melt blending and extrusion is 200-240°C and the rotation speed is 200-400r / min.

[0054] Example 5

[0055] Preparation of PLA / ABS composites:

[0056] Prepare the following raw materials in parts by weight: 90 parts of PLA resin, 10 parts of ABS resin, 10 parts of the auxiliary agent prepared in Example 1, and 1.5 parts of a nucleating agent; the nucleating agent is a mixture of TMC-300 and carbon nanotubes in a mass ratio of 3:1;

[0057] Melt extrusion: PLA resin, ABS resin, additives and nucleating agents are mixed, melt blended and extruded, and granulated to obtain a composite material, wherein the temperature during the melt blending and extrusion is 200-240°C and the rotation speed is 200-400r / min.

[0058] Comparative Example 1

[0059] Preparation of PLA / ABS composite material: Compared with Example 5, the additive in Example 5 was replaced by the modified polydimethylsiloxane prepared in Example 1, and the rest was the same.

[0060] Comparative Example 2

[0061] Preparation of PLA / ABS composite material: Compared with Example 5, the same amount of the auxiliary agent in Example 5 was replaced by the following steps to prepare polycaprolactone, and the rest was the same:

[0062] 0.4 g of stannous isooctanoate was added to 5 g of caprolactone under nitrogen atmosphere and 90°C with stirring, and the reaction was continued with heat preservation and stirring for 24 hours. The reaction was stopped and the product was repeatedly treated with dichloromethane and isopropanol system (dispersion, precipitation, washing, centrifugation) and finally dried to obtain polycaprolactone.

[0063] Comparative Example 3

[0064] Preparation of PLA / ABS composite material: Compared with Example 5, the additive in Example 5 was replaced by maleic anhydride grafted ABS, and the rest was the same.

[0065] Comparative Example 4

[0066] Preparation of PLA / ABS composite material: Compared with Example 5, the nucleating agent in Example 5 was deleted, and the rest was the same.

[0067] The composite materials obtained in Examples 3-5 and Comparative Examples 1-4 were tested for physical properties, and the results are shown in Table 1.

[0068] Table 1

[0069] Tensile Strength Bending Strength Notched impact strength Flame retardant grade Heat Deflection Temperature GB / T 1040.2 GB / T 9341 GB / T 1043.1 UL-94 ISO 75-2 unit Mpa Mpa <![CDATA[KJ / m 2 ]]> / ℃ Example 3 76 104 16.8 V-1 117 Example 4 63 94 16.2 V-1 113 Example 5 60 91 15.1 V-1 109 Comparative Example 1 41 72 11.3 V-1 104 Comparative Example 2 45 70 12.5 V-2 95 Comparative Example 3 47 82 13.5 V-2 92 Comparative Example 4 57 89 12.7 V-1 101

[0070] From the data in Table 1, it can be seen that the composite materials obtained in Examples 3-5 have good mechanical strength, toughness and thermal stability, and have certain flame retardant properties.

[0071] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0072] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A bio-based toughened flame-retardant PLA / ABS composite material, characterized in that: The method comprises the following raw materials in parts by weight: 75-90 parts of PLA resin, 10-25 parts of ABS resin, 10-20 parts of auxiliary agent, and 0.5-1.5 parts of nucleating agent; The auxiliary agent is prepared by a ring-opening polymerization reaction of modified polydimethylsiloxane and caprolactone under the action of a ring-opening catalyst; The modified polydimethylsiloxane is prepared by reacting bisaminopropyl polydimethylsiloxane with a reactive weather-resistant compound.

2. The bio-based toughened flame-retardant PLA / ABS composite material according to claim 1, characterized in that: The reaction conditions of the ring-opening polymerization reaction are: a reaction temperature of 90-130° C. and a reaction time of 12-48 hours under a nitrogen atmosphere.

3. The bio-based toughened flame-retardant PLA / ABS composite material according to claim 1, characterized in that: The mass ratio of the modified polydimethylsiloxane to caprolactone is 15-25:5-8.

4. The bio-based toughened flame-retardant PLA / ABS composite material according to claim 1, characterized in that: The ring-opening catalyst is one of stannous isooctanoate, dibutyltin dilaurate, trifluoromethanesulfonic acid and hydrofluoric acid.

5. The bio-based toughened flame-retardant PLA / ABS composite material according to claim 1, characterized in that: The reaction conditions for obtaining the modified polydimethylsiloxane are: reaction temperature of 0-20° C., and reaction time of 3-8 h.

6. The bio-based toughened flame-retardant PLA / ABS composite material according to claim 1, characterized in that: The mass ratio of the bisaminopropyl polydimethylsiloxane to the reactive weather-resistant compound is 15-25:

3.

7. The bio-based toughened flame-retardant PLA / ABS composite material according to claim 1, characterized in that: The number average molecular weight of the bisaminopropyl polydimethylsiloxane is 1000-2000.

8. The bio-based toughened flame-retardant PLA / ABS composite material according to claim 1, characterized in that: The reactive weather-resistant compound is prepared by reacting chloroacetyl chloride and 2,4-dihydroxybenzophenone in the presence of an organic solvent and an acid-binding agent.

9. The bio-based toughened flame-retardant PLA / ABS composite material according to claim 1, characterized in that: The nucleating agent is a mixture of an organic nucleating agent and an inorganic nucleating agent in a mass ratio of 2-3:

1.

10. A method for preparing a bio-based toughened flame-retardant PLA / ABS composite material according to any one of claims 1 to 9, characterized in that: include: The PLA resin, ABS resin, auxiliary agent and nucleating agent are mixed, melt-blended, extruded and granulated to obtain a composite material.

Citation Information

Patent Citations

  • Bio-based toughened flame-retardant PLA / ABS composite material and preparation method thereof

    CN112662150A

  • Regenerated modified plastic based on waste plastic

    CN114479429A

  • Flame-retardant high-toughness PLA alloy material, and preparation method therefor and use thereof