Fire-resistant flame-retardant porcelainized polysiloxane foam material and preparation method thereof
By cross-linking to form a dense porous structure and ceramic layer, polysiloxane foam materials solve the problem of insufficient flame retardant performance in existing technologies, achieving lower ceramic forming temperature and better fire resistance and flame retardant effect.
Patent Information
- Application Number
- CN202411178528.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
Existing polysiloxane foam materials have insufficient flame retardant and fire-resistant properties to meet high requirements, and their high ceramicization temperature makes them unable to effectively prevent the spread of flames.
A dense porous structure is formed by cross-linking methyl vinyl-terminated organopolysiloxanes, polymethylhydrosiloxanes, and hydroxyl polysiloxanes. Halogen-free flame retardants and ceramic fillers are added, and the cross-linking reaction is promoted by a catalyst to form a hard ceramic layer to prevent the spread of flames.
It improves the flame retardant and fire-resistant properties of polysiloxane foam materials, reduces the ceramic forming temperature, and enables the structure to maintain its integrity in high-temperature environments, effectively slowing the spread of fire.
Smart Images

Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material and a preparation method thereof. Background Art
[0002] Foam materials have been widely used in all aspects of life and have become one of the indispensable materials in life. Soft foam materials are mainly used in household products such as sofas, chairs, pillows, mattresses, insoles, etc.; hard foam materials are mainly used in thermal insulation and building fire insulation and other caulking materials. Addition-type polysiloxane foam is odorless, and its combustion decomposition products are low-toxic and harmless SiO2, CO2, H2O and other substances. It shows excellent properties such as acid resistance, alkali resistance, corrosion resistance, flame resistance, radiation resistance, high and low temperature resistance, biocompatibility and electrical insulation. At the same time, it also has excellent properties such as low density, high elasticity, good sound insulation and thermal insulation, which makes it have broad application prospects in many fields such as daily necessities, medical treatment, aerospace, building materials, aviation, etc.
[0003] In the prior art, polysiloxane foam is modified to obtain a ceramic polysiloxane foam material, which has good fire resistance and can be ceramicized at high temperature to prevent the spread of flames.
[0004] For example, the Chinese invention with the announcement number CN113122180A discloses a fire-resistant and ceramicizable organic silicon foam sealant, including component A and component B. Component A includes terminal hydroxyl polysiloxane, white carbon black, polysilazane resin, hydrogenated silicone oil, ceramic filler, aluminum-based aerogel, and reaction inhibitor. Component B includes terminal hydroxyl polysiloxane, white carbon black, hydroxyl silicone oil, ceramic filler, and catalyst. The terminal hydroxyl polysiloxane and hydrogenated silicone oil are condensed and dehydrogenated to form the main body of the organic silicon foam sealant, and the main body of the organic silicon foam sealant has certain flame retardant properties, and has fireproof, flame retardant and heat insulation properties through the synergistic effect of polysilazane resin, homemade aluminum-based aerogel and ceramic filler.
[0005] For example, the Chinese invention with announcement number CN116715951A discloses a ceramicizable halogen-free flame-retardant thermoplastic polyurethane elastomer, including a thermoplastic polyurethane elastomer, a terminal hydroxyl polysiloxane, a non-flame retardant, a ceramic filler, a foaming cross-linking agent, an antioxidant, and other additives. When the temperature is greater than 700°C, the thermoplastic polyurethane elastomer forms a complete foam ceramic layer to achieve a fire-resistant function.
[0006] However, as people have higher and higher requirements for the flame retardancy and flame resistance of foam materials, in order to meet people's demand for highly flame retardant and flame resistant foam materials, the present invention proposes a fire-resistant and flame-retardant porcelain-able polysiloxane foam material, which has a lower porcelain forming temperature and a more fire-resistant and flame-retardant foam material body, thereby achieving a more excellent fire-resistant and flame-retardant effect. Summary of the invention
[0007] In order to overcome the shortcomings of the above-mentioned technology, the present invention provides a fire-resistant and flame-retardant porcelain-forming polysiloxane foam material, which has excellent fire-resistant and flame-retardant properties and a low porcelain-forming temperature. It can maintain the integrity of the structure under high temperature environment, effectively slow down the spread of fire when a fire occurs, and reduce the degree of fire damage.
[0008] To achieve the above-mentioned purpose, the present invention provides a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, comprising the following raw materials in parts by weight: 100 parts of silicone rubber base, 10 to 20 parts of hydroxy polysiloxane, 10 to 20 parts of polymethyl hydrogen siloxane, 1 to 2 parts of catalyst, 10 to 20 parts of non-ionic surfactant, 2 to 4 parts of inhibitor, 0 to 60 parts of flux, 20 to 105 parts of porcelain-forming filler, 20 to 40 parts of halogen-free flame retardant, 1 to 2 parts of colorant, and 0 to 6 parts of foaming agent; at least one end group of the polymethyl hydrogen siloxane is Si-H; and the hydroxy polysiloxane is terminated by hydroxyl groups.
[0009] Preferably, the mass fraction of methyl vinyl in the silicone rubber base is 0.03-2%, the mass fraction of Si-H in the polymethylhydrogensiloxane is 0.5-2%, and the mass fraction of hydroxyl in the hydroxypolysiloxane is 0.5-5%.
[0010] Preferably, at 25° C., the viscosity of the silicone rubber base is 350 to 2,000,000 mPa·s, the viscosity of the hydroxy polysiloxane is 1,000 to 3,000 mPa·s, and the viscosity of the polymethyl hydrogen siloxane is 500 to 1,000 mPa·s.
[0011] Preferably, the silicone rubber base includes white carbon black, and the silicone rubber base is a mixed rubber.
[0012] Preferably, the catalyst is one of platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, dichlorobis(chlorocyclohexene)platinum (II), tetrakis(triphenylphosphine)platinum (0), and chloroplatinic acid (IV) isopropanol; and the inhibitor is one of triphenyl phosphite, tri-tert-butyl phosphite, and triethyl phosphite.
[0013] Preferably, the nonionic surfactant is one of anhydrous sorbitan fatty acid ester, polyoxyethylene fatty alcohol ether, alkylphenol polyoxyethylene ether, and polyol polyoxyethylene ether fatty acid ester.
[0014] Preferably, the melting point of the flux is 500-1500°C, and the flux includes at least one of boron glass beads, potassium-containing glass beads, and high-silicon glass beads; the porcelain-forming filler is at least one of diatomaceous earth, glass fiber powder, kaolin, forsterite, wollastonite, mica, phlogopite, mullite, and ceramic composite powder.
[0015] Preferably, the halogen-free flame retardant includes at least one of silicon dioxide, boron nitride, boron carbide, molybdenum disulfide, expanded graphite, silicon powder, silicon carbide, silicon nitride, zinc borate, zinc aluminate, metal oxides or metal hydroxides; wherein the metal oxides or hydroxides include magnesium oxide, aluminum oxide, zinc oxide, iron oxide, zirconium oxide, molybdenum oxide, cerium oxide and other lanthanide oxides and the hydroxides corresponding to each oxide.
[0016] To achieve the above object, the present invention further provides a method for preparing a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, comprising the following steps:
[0017] Step 1: Add methyl vinyl terminated polysiloxane and white carbon black into an internal mixer, stir at a stirring speed of 800 to 1000 r / min at 130° C. for 50 to 60 minutes to obtain a silicone rubber base;
[0018] Step 2: Add hydroxy polysiloxane, nonionic surfactant, colorant, flux, porcelain filler and halogen-free flame retardant into an internal mixer in sequence, and stir at room temperature for 30 to 50 minutes at a stirring speed of 800 to 1000 r / min to obtain a mixture;
[0019] Step 3: Add the inhibitor and polymethylhydrogensiloxane into an internal mixer, stir at a stirring speed of 200 to 400 r / min for 20 to 30 minutes, cool to room temperature, and cut into samples with a thickness of 1 to 3 mm;
[0020] Step 4: Mix the sample with the catalyst and vulcanize at 50-100° C. for 10-30 minutes; then heat to 150° C. and vulcanize for 30-60 minutes to obtain a fire-resistant, flame-retardant, ceramic polysiloxane foam material.
[0021] Preferably, a foaming aid is added in step 2.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The main body of the polysiloxane foam material of the present invention is formed by cross-linking an organic polysiloxane terminated with methyl vinyl, a polymethyl hydrogen siloxane and a hydroxy polysiloxane. The vinyl group on the organic polysiloxane terminated with methyl vinyl and Si-H on the polymethyl hydrogen siloxane form a cross-linked network structure through an addition reaction, and the hydroxyl group on the hydroxy polysiloxane and Si-H on the polymethyl hydrogen siloxane form a network structure through a dehydrogenation condensation reaction. This structure enables the main body of the polysiloxane foam material to have a relatively dense pore structure. The dense pore structure effectively reduces the heat conduction path inside the material, thereby improving the heat resistance of the polysiloxane foam material.
[0024] 2. The dehydrogenation condensation of hydroxy polysiloxane and polymethyl hydrogen siloxane produces hydrogen, which makes the material form a uniform and dense pore structure with a comfortable feel.
[0025] 3. When the surface of the polysiloxane foam material contacts the flame, the Si-O structure of the organic polysiloxane, polymethyl hydrogen siloxane and hydroxy polysiloxane will produce silicon dioxide to prevent further burning of the flame, thereby enhancing the flame retardant properties of the main body of the polysiloxane foam material.
[0026] 4. Halogen-free flame retardants can promote the melting of flux. At 400-700°C, the flux melts and forms a hard and continuous ceramic layer with the ceramic filler. This ceramic layer has a heat-insulating effect, effectively preventing flames or high temperatures from being transmitted into the material, and preventing flames from spreading into the polysiloxane foam material, so that the polysiloxane foam material can have flame-retardant properties at low ignition temperatures.
[0027] 5. Non-ionic surfactants are used to make flux, ceramic filler, halogen-free flame retardant compatible with organic polysiloxane, polymethyl hydrogen siloxane, hydroxy polysiloxane, and the surfactant will not affect the action of the catalyst. Flux can enhance the fluidity of ceramic filler, and promote it to form a continuous, smooth, crack-free ceramic layer on the surface of polysiloxane foam material. The crack-free ceramic layer can effectively prevent the penetration and spread of flames, thereby further improving the flame retardant properties of the material. DETAILED DESCRIPTION
[0028] The features of the present invention and other related features are further described in detail below through embodiments to facilitate understanding by those skilled in the art:
[0029] The embodiment of the present invention provides a fire-resistant, flame-retardant, porcelain-forming polysiloxane foam material, comprising the following raw materials in parts by weight: 100 parts of silicone rubber base, 10 to 20 parts of hydroxy polysiloxane, 10 to 20 parts of polymethyl hydrogen siloxane, 1 to 2 parts of catalyst, 10 to 20 parts of non-ionic surfactant, 2 to 4 parts of inhibitor, 0 to 60 parts of flux, 20 to 105 parts of porcelain-forming filler, 20 to 40 parts of halogen-free flame retardant, 1 to 2 parts of colorant, and 0 to 6 parts of foaming agent; at least one end group of the polymethyl hydrogen siloxane is Si-H; and the hydroxy polysiloxane is terminated by hydroxyl groups.
[0030] In some embodiments, the mass fraction of methyl vinyl in the silicone rubber base is 0.03-2%, the mass fraction of Si-H in the polymethylhydrogensiloxane is 0.5-2%, and the mass fraction of hydroxyl in the hydroxypolysiloxane is 0.5-5%.
[0031] In some embodiments, at 25° C., the viscosity of the silicone rubber base is 350 to 2,000,000 mPa·s, the viscosity of the hydroxy polysiloxane is 1,000 to 3,000 mPa·s, and the viscosity of the polymethyl hydrogen siloxane is 500 to 1,000 mPa·s.
[0032] In some embodiments, the silicone rubber base includes white carbon black, which can improve the flame retardant performance and thermal stability of the silicone rubber base. The silicone rubber base is a mixed rubber.
[0033] In some embodiments, the catalyst is one of platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, dichlorobis(chlorocyclohexene)platinum (II), tetrakis(triphenylphosphine)platinum (0), and chloroplatinic acid (IV) isopropanol.
[0034] In some embodiments, since the catalyst causes the hydroxy polysiloxane and the polymethyl hydrogen siloxane to undergo rapid dehydrogenation condensation, and the methyl vinyl of the organopolysiloxane reacts with the Si-H of the polymethyl hydrogen siloxane, an inhibitor is added to the polysiloxane foam material to prevent the reaction from being too intense and causing violent polymerization. The inhibitor is one of triphenyl phosphite, tri-tert-butyl phosphite, and triethyl phosphite.
[0035] In some embodiments, the nonionic surfactant is one of anhydrous sorbitan fatty acid ester, polyoxyethylene fatty alcohol ether, alkylphenol polyoxyethylene ether, and polyol polyoxyethylene ether fatty acid ester.
[0036] In some embodiments, the melting point of the flux is 500-1500°C, and the flux includes at least one of boron glass beads, potassium-containing glass beads, and high-silicon glass beads; the porcelain-forming filler is at least one of diatomaceous earth, glass fiber powder, kaolin, forsterite, wollastonite, mica, phlogopite, and mullite.
[0037] In some embodiments, the halogen-free flame retardant includes at least one of silicon dioxide, boron nitride, boron carbide, molybdenum disulfide, expanded graphite, silicon powder, silicon carbide, silicon nitride, zinc borate, zinc aluminate, metal oxides or metal hydroxides; wherein the metal oxides or hydroxides include magnesium oxide, aluminum oxide, zinc oxide, iron oxide, zirconium oxide, molybdenum oxide, cerium oxide and other lanthanide oxides and the hydroxides corresponding to each oxide.
[0038] The embodiment of the present invention also provides a method for preparing a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, comprising the following steps:
[0039] Step 1: Add methyl vinyl terminated polysiloxane and white carbon black into an internal mixer, stir at a stirring speed of 800 to 1000 r / min at 130° C. for 50 to 60 minutes to obtain a silicone rubber base.
[0040] Step 2: Add hydroxy polysiloxane, nonionic surfactant, colorant, flux, porcelain filler and halogen-free flame retardant into an internal mixer in sequence, stir at a stirring speed of 800 to 1000 r / min at room temperature for 30 to 50 minutes to obtain a mixture.
[0041] Step 3: Add the inhibitor and polymethylhydrogensiloxane into an internal mixer, stir at a stirring speed of 200 to 400 r / min for 20 to 30 minutes, cool to room temperature, and cut into samples with a thickness of 1 to 3 mm.
[0042] Step 4: Mix the sample with the catalyst and vulcanize at 50-100° C. for 10-30 minutes; then heat to 150° C. and vulcanize for 30-60 minutes to obtain a fire-resistant, flame-retardant, ceramic polysiloxane foam material.
[0043] In some embodiments, when the Si-H dehydrogenation condensation of hydroxy polysiloxane and polymethyl hydrogen siloxane produces too little hydrogen, a foaming aid may be added. The foaming aid is one or more of water, methanol, ethanol, α,ω-diol, 1,4-butanediol, and 1,5-pentanediol.
[0044] Embodiment 1 of the present invention provides a method for preparing a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, which comprises the following steps:
[0045] Step 1: Add 100g of methyl vinyl terminated polysiloxane and 50g of white carbon black into an internal mixer, stir at a stirring speed of 800-1000r / min at 130°C for 50-60min to obtain a silicone rubber base, and retain 100g of the silicone rubber base in the internal mixer.
[0046] Step 2: Add 10g of hydroxypolysiloxane, 10g of anhydrous sorbitan fatty acid ester Span-20, 2g of black colorant, 40g of solid borosilicate glass beads, 20g of diatomaceous earth, 10g of aluminum hydroxide, 10g of aluminum oxide, and 4g of methanol into an internal mixer in sequence, and stir at room temperature for 30 to 50min at a stirring speed of 800 to 1000r / min to obtain a mixture.
[0047] Step 3: Add 2 g of 1-ethynylcyclopentanol and 10 g of polymethylhydrogensiloxane into an internal mixer, stir at a stirring speed of 200 to 400 r / min for 20 to 30 min, cool to room temperature, and cut into samples with a thickness of 2 mm.
[0048] Step 4: Mix the sample with 1 g of tetrakis(triphenylphosphine)platinum(0), and vulcanize at 50-100° C. for 10-30 min; then heat to 150° C. and vulcanize for 30-60 min to obtain a fire-resistant, flame-retardant, ceramic polysiloxane foam material.
[0049] Embodiment 2 of the present invention provides a method for preparing a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, which comprises the following steps:
[0050] Step 1: Add 100g of methyl vinyl terminated polysiloxane and 50g of white carbon black into an internal mixer, stir at a stirring speed of 800-1000r / min at 130°C for 50-60min to obtain a silicone rubber base, and retain 100g of the silicone rubber base in the internal mixer.
[0051] Step 2: Add 10g of hydroxypolysiloxane, 15g of anhydrous sorbitan fatty acid ester Span-80, 2g of black colorant, 40g of solid borosilicate glass beads, 20g of mica, 30g of magnesium hydroxide, 10g of aluminum hydroxide, and 4g of methanol into an internal mixer in sequence, and stir at room temperature for 30 to 50min at a stirring speed of 800 to 1000r / min to obtain a mixture.
[0052] Step 3: Add 2 g of 1-ethynylcyclopentanol and 10 g of polymethylhydrogensiloxane into an internal mixer, stir at a stirring speed of 200 to 400 r / min for 20 to 30 min, cool to room temperature, and cut into samples with a thickness of 2 mm.
[0053] Step 4: Mix the sample with 1 g of tetrakis(triphenylphosphine)platinum(0), and vulcanize at 50-100° C. for 10-30 min; then heat to 150° C. and vulcanize for 30-60 min to obtain a fire-resistant, flame-retardant, ceramic polysiloxane foam material.
[0054] Embodiment 3 of the present invention provides a method for preparing a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, which comprises the following steps:
[0055] Step 1: Add 100g of methyl vinyl terminated polysiloxane and 50g of white carbon black into an internal mixer, stir at a stirring speed of 800-1000r / min at 130°C for 50-60min to obtain a silicone rubber base, and retain 100g of the silicone rubber base in the internal mixer.
[0056] Step 2: Add 10g of hydroxypolysiloxane, 20g of anhydrous sorbitan fatty acid ester Span-80, 2g of black colorant, 60g of solid borosilicate glass beads, 20g of wollastonite, 15g of zinc borate, 15g of aluminum hydroxide, and 4g of methanol into an internal mixer in sequence, and stir at room temperature for 30 to 50min at a stirring speed of 800 to 1000r / min to obtain a mixture.
[0057] Step 3: Add 2 g of 1-ethynylcyclopentanol and 20 g of polymethylhydrogensiloxane into an internal mixer, stir at a stirring speed of 200 to 400 r / min for 20 to 30 min, cool to room temperature, and cut into samples with a thickness of 2 mm.
[0058] Step 4: Mix the sample with 1 g of tetrakis(triphenylphosphine)platinum(0), and vulcanize at 50-100° C. for 10-30 min; then heat to 150° C. and vulcanize for 30-60 min to obtain a fire-resistant, flame-retardant, ceramic polysiloxane foam material.
[0059] Embodiment 4 of the present invention provides a method for preparing a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, which comprises the following steps:
[0060] Step 1: Add 100g of methyl vinyl terminated polysiloxane and 50g of white carbon black into an internal mixer, stir at a stirring speed of 800-1000r / min at 130°C for 50-60min to obtain a silicone rubber base, and retain 100g of the silicone rubber base in the internal mixer.
[0061] Step 2: Add 10g of hydroxypolysiloxane, 20g of anhydrous sorbitan fatty acid ester Span-40, 2g of black colorant, 60g of solid borosilicate glass beads, 20g of ceramic powder, 5g of expandable graphite, 15g of aluminum hydroxide, and 6g of methanol into an internal mixer in sequence, and stir at room temperature for 30 to 50min at a stirring speed of 800 to 1000r / min to obtain a mixture.
[0062] Step 3: Add 2 g of 1-ethynylcyclopentanol and 20 g of polymethylhydrogensiloxane into an internal mixer, stir at a stirring speed of 200 to 400 r / min for 20 to 30 min, cool to room temperature, and cut into samples with a thickness of 2 mm.
[0063] Step 4: Mix the sample with 1 g of tetrakis(triphenylphosphine)platinum(0), and vulcanize at 50-100° C. for 10-30 min; then heat to 150° C. and vulcanize for 30-60 min to obtain a fire-resistant, flame-retardant, ceramic polysiloxane foam material.
[0064] Embodiment 5 of the present invention provides a method for preparing a fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, which comprises the following steps:
[0065] Step 1: Add 100g of methyl vinyl terminated polysiloxane and 50g of white carbon black into an internal mixer, stir at a stirring speed of 800-1000r / min at 130°C for 50-60min to obtain a silicone rubber base, and retain 100g of the silicone rubber base in the internal mixer.
[0066] Step 2: Add 10g of hydroxypolysiloxane, 20g of anhydrous sorbitan fatty acid ester Span-40, 2g of black colorant, 80g of ceramic composite powder, 25g of mica powder, 15g of aluminum hydroxide, and 6g of water into an internal mixer in sequence, and stir at room temperature for 30 to 50 minutes at a stirring speed of 800 to 1000 r / min to obtain a mixture.
[0067] Step 3: Add 2 g of 1-ethynylcyclopentanol and 20 g of polymethylhydrogensiloxane into an internal mixer, stir at a stirring speed of 200 to 400 r / min for 20 to 30 min, cool to room temperature, and cut into samples with a thickness of 2 mm.
[0068] Step 4: Mix the sample with 1 g of tetrakis(triphenylphosphine)platinum(0), and vulcanize at 50-100° C. for 10-30 min; then heat to 150° C. and vulcanize for 30-60 min to obtain a fire-resistant, flame-retardant, ceramic polysiloxane foam material.
[0069] Comparative Example 1 of the present invention provides a polysiloxane foam material. Compared with Example 3, the polysiloxane foam material of Comparative Example 1 does not contain zinc borate or aluminum hydroxide.
[0070] Comparative Example 2 of the present invention provides a polysiloxane foam material. Compared with Example 5, the polysiloxane foam material of Comparative Example 2 does not contain any ceramic composite powder.
[0071] 1. Determination of apparent density of polysiloxane foam materials according to GB / T 6343-2009 standard
[0072] 2. According to GB / T 6669-2008 standard, the compression permanent deformation percentage of polysiloxane foam material is measured. The polysiloxane foam material is pressed with a heavy object and placed at 150°C for 168 hours. According to the formula Calculated, where d0 is the initial height (mm), d1 is the height after compression (mm), and d2 is the rebound height (mm).
[0073] 3. The tensile strength and elongation at break of polysiloxane foam materials were determined according to GB / T 6344-2008.
[0074] 4. Determine the flame retardancy level of polysiloxane foam materials according to UL94 standard.
[0075] Table 1 Test results of embodiments and comparative examples
[0076]
[0077]
[0078] (1) It can be seen from Examples 1 to 5 and Comparative Example 2 that the polysiloxane foam material can be ceramicized at high temperatures and has better flame retardant properties. Compared with Example 5, Comparative Example 2 lacks ceramic composite powder and has no flux to assist mica in ceramicization, resulting in a flame retardant level of only UL94V-3 for Comparative Example 2. The ceramic composite powder of Example 5 has excellent ceramic-forming properties, so it can be ceramicized without adding flux.
[0079] (2) Comparison of Examples 1 to 2 and Example 3 with Comparative Example 1 shows that a small amount of halogen-free flame retardant added to the polysiloxane foam material will reduce its flame retardant properties, and the mechanical properties of the polysiloxane foam material will also decrease as the mass of the halogen-free flame retardant decreases. Comparison of Example 5 with Comparative Example 2 shows that the ceramic filler can also improve the mechanical properties of the polysiloxane foam material.
[0080] (3) As can be seen from Examples 1 to 5, the apparent density of the polysiloxane foam material of the present invention is 0.34 to 0.56 g / cm 3 , between medium foaming and low foaming, with excellent mechanical properties, and the flame retardant level of Examples 2 to 5 reaches UL94 V-0, and can be applied to the field of filling foam materials for battery packs, household appliances, building fireproof materials, and wire and cable sheaths.
[0081] (4) Although Example 1 cannot be formed into porcelain, its flame retardant level can still reach UL94 V-1. This is because the polysiloxane foam material has excellent flame retardant properties, and the halogen-free flame retardant releases water vapor when ignited, lowers the temperature, and forms an isolation layer with a higher melting point, which can slow down the spread of fire.
[0082] (5) As can be seen from Examples 1 to 5, since nonionic surfactants are used to make flux compatible with organic polysiloxane, polymethyl hydrogen siloxane and hydroxy polysiloxane, as the flux in the polysiloxane foam increases, the nonionic surfactant also needs to be increased accordingly.
[0083] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structural transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, is also included in the patent protection scope of the present invention.
Claims
1. A fire-resistant, flame-retardant, porcelainizable polysiloxane foam material, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of silicone rubber base, 10 to 20 parts of hydroxy polysiloxane, 10 to 20 parts of polymethyl hydrogen siloxane, 1 to 2 parts of catalyst, 10 to 20 parts of nonionic surfactant, 2 to 4 parts of inhibitor, 0 to 60 parts of flux, 20 to 105 parts of porcelain-forming filler, 20 to 40 parts of halogen-free flame retardant, 1 to 2 parts of colorant and 0 to 6 parts of foaming agent; the silicone rubber base comprises methyl vinyl terminated organic polysiloxane; at least one end group of the polymethyl hydrogen siloxane is Si-H; the hydroxy polysiloxane is terminated by hydroxyl group.
2. The fire-resistant, flame-retardant, porcelainizable polysiloxane foam material according to claim 1, characterized in that: The mass fraction of methyl vinyl in the silicone rubber base is 0.03-2%, the mass fraction of Si-H in the polymethyl hydrogen siloxane is 0.5-2%, and the mass fraction of hydroxyl in the hydroxy polysiloxane is 0.5-5%.
3. The fire-resistant, flame-retardant, porcelainizable polysiloxane foam material according to claim 1, characterized in that: At 25° C., the viscosity of the silicone rubber base is 350 to 2,000,000 mPa·s, the viscosity of the hydroxy polysiloxane is 1,000 to 3,000 mPa·s, and the viscosity of the polymethyl hydrogen siloxane is 500 to 1,000 mPa·s.
4. The fire-resistant, flame-retardant, porcelainizable polysiloxane foam material according to claim 1, characterized in that: The silicone rubber base includes white carbon black, and the silicone rubber base is a mixed rubber.
5. The fire-resistant, flame-retardant, porcelainizable polysiloxane foam material according to claim 1, characterized in that: The catalyst is one of platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, dichlorobis(chlorocyclohexene)platinum (II), tetrakis(triphenylphosphine)platinum (0), and chloroplatinic acid (IV) isopropanol solution; the inhibitor is one of triphenyl phosphite, tri-tert-butyl phosphite, and triethyl phosphite.
6. The fire-resistant, flame-retardant, porcelainizable polysiloxane foam material according to claim 1, characterized in that: The nonionic surfactant is one of anhydrous sorbitan fatty acid ester, polyoxyethylene fatty alcohol ether, alkylphenol polyoxyethylene ether, and polyol polyoxyethylene ether fatty acid ester.
7. The fire-resistant, flame-retardant, porcelainizable polysiloxane foam material according to claim 1, characterized in that: The melting point of the flux is 500-1500° C., and the flux includes at least one of boron glass beads, potassium-containing glass beads, and high-silicon glass beads; the ceramic filler is at least one of diatomaceous earth, glass fiber powder, kaolin, forsterite, wollastonite, mica, phlogopite, mullite, and ceramic composite powder.
8. The fire-resistant, flame-retardant, porcelainizable polysiloxane foam material according to claim 7, characterized in that: The halogen-free flame retardant includes at least one of silicon dioxide, boron nitride, boron carbide, molybdenum disulfide, expanded graphite, silicon powder, silicon carbide, silicon nitride, zinc borate, zinc aluminate, metal oxides or metal hydroxides; wherein the metal oxides or hydroxides include magnesium oxide, aluminum oxide, zinc oxide, iron oxide, zirconium oxide, molybdenum oxide, cerium oxide and other lanthanide oxides and the hydroxides corresponding to each oxide; the particle pore sizes of the ceramic filler, flux and halogen-free flame retardant are all 1000-5000 meshes.
9. A method for preparing a fire-resistant, flame-retardant, porcelain-able polysiloxane foam material, for preparing the fire-resistant, flame-retardant, porcelain-able polysiloxane foam material according to any one of claims 1 to 8, comprising the following steps: Step 1: Add methyl vinyl terminated polysiloxane and white carbon black into an internal mixer, stir at a stirring speed of 800 to 1000 r / min at 130° C. for 50 to 60 minutes to obtain a silicone rubber base; Step 2: Add hydroxy polysiloxane, nonionic surfactant, colorant, flux, porcelain filler and halogen-free flame retardant into an internal mixer in sequence, and stir at room temperature for 30 to 50 minutes at a stirring speed of 800 to 1000 r / min to obtain a mixture; Step 3: Add the inhibitor and polymethylhydrogensiloxane into an internal mixer, stir at a stirring speed of 200 to 400 r / min for 20 to 30 minutes, cool to room temperature, and cut into samples with a thickness of 1 to 3 mm; Step 4: Mix the sample with the catalyst and vulcanize at 50-100° C. for 10-30 minutes; then heat to 150° C. and vulcanize for 30-60 minutes to obtain a fire-resistant, flame-retardant, ceramic polysiloxane foam material.
10. The fire-resistant, flame-retardant, porcelainizable polysiloxane foam material according to claim 9, characterized in that: In the step 2, a foaming aid is added.
Citation Information
Patent Citations
Fireproof ceramizable organosilicon foaming sealant and preparation method thereof
CN113122180A
Porcelainized halogen-free flame-retardant thermoplastic polyurethane elastomer and preparation method thereof
CN116715951A