Liquid rubber modifier / SBS composite modified asphalt and preparation method thereof
Through liquid rubber modifier/SBS composite modified asphalt technology, the problems of high-temperature operations, easy separation and environmental pollution in traditional rubber asphalt processing have been solved, and the stability and economicality of asphalt have been improved. It is suitable for highway construction and has reduced the Environmentally friendly pollution.
Patent Information
- Application Number
- CN202410959169.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
AI Technical Summary
The traditional rubber asphalt processing methods have problems such as high-temperature operations, complex equipment, high energy consumption, easy to separate products, difficult construction, easy to produce asphalt smoke and rubber odor, strict construction temperature control, and poor economicality, resulting in reduced performance of asphalt roads and Environmentally friendly pollution.
Using liquid rubber modifier/SBS composite modified asphalt technology, the waste tire powder is converted into liquid rubber modifier and the base asphalt reacts and swells fully. The mixing temperature is controlled at 160-170℃ to prevent asphalt aging and during construction SBS was introduced to improve the compatibility and ease of asphalt.
It solves the problems of easy separation and high-temperature aging of rubber asphalt, improves the construction performance and economy of asphalt, reduces environmental pollution, and improves the stability and applicability of asphalt.
Smart Images

Figure CN118931212A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of modified asphalt, and in particular to a liquid rubber modifier / SBS composite modified asphalt and a preparation method thereof. Background Art
[0002] In recent years, the development of the automobile industry has driven the rapid progress of the rubber industry, and the number of waste tires has been increasing at a rate of 8%-10% per year. Waste tires cannot be naturally degraded or split, so they cannot be simply landfilled; if they are burned, they will produce a large amount of toxic gases and pollute the environment; at the same time, waste tires occupy land resources, are prone to breeding mosquitoes, and are prone to fire. Treating waste tires in a certain way and using them in highway construction is not only beneficial to the environment, but also can save highway construction funds.
[0003] According to investigations and studies, there are two main traditional modification and processing techniques for rubber asphalt mixtures: the "dry method" and the "wet method". The "dry method" is to add waste tire rubber powder directly into the asphalt mixture as a filler, without modifying the properties of the asphalt, resulting in reduced asphalt road performance. The "wet method" is usually to mix, swell, and high-speed shear grind the waste tire rubber powder with the base asphalt under high temperature, so that the waste tire rubber powder is evenly dispersed in the asphalt in a certain particle size. The waste tire rubber powder is fully swelled in the asphalt, which improves the performance of the base asphalt. The "wet method" is currently the method commonly used in China. However, during engineering use, rubber asphalt processed by the "wet method" has the following disadvantages:
[0004] 1. The processing is difficult, the equipment used is complex, and the energy consumption is high, which increases the production cost of asphalt mixture.
[0005] 2. Rubber asphalt is prone to segregation during storage and transportation, which affects product quality. There is only partial adsorption and solubility between waste tire rubber powder and asphalt, but not complete fusion. This system is a thermodynamically unstable system, which is very easy to separate the two and cause segregation. In addition, once the physical modified asphalt product processed on site stops stirring, the waste tire rubber powder will separate from the asphalt and float on the surface to condense, forming a rough surface with larger particles. Therefore, physical modified asphalt is produced and spread on site, and the product is not easy to store.
[0006] 3. The processing temperature is high and the asphalt is prone to aging. The processing temperature of "wet process" rubber asphalt is generally between 180℃ and 200℃, and the processing time is relatively long, so the quality of modified asphalt is very easy to decay.
[0007] 4. During on-site processing, due to high-temperature operations, a large amount of asphalt smoke and rubber odor are generated, which is unpleasant and pungent, causing physical harm to on-site operators and pollution to the surrounding environment.
[0008] 5. The construction and workability of rubber asphalt is relatively poor, and the temperature control during construction is more stringent, which brings difficulties to the construction.
[0009] 6. It is only applicable to discontinuous grading or open grading, which results in large asphalt consumption and poor economy.
[0010] In this regard, domestic and foreign scholars have proposed many methods, such as: in order to solve the problem of poor high temperature, a composite modification method is used to add SBS and other modifiers to rubber asphalt; in order to solve the asphalt aging problem caused by high construction temperature, a warm mix agent is added to reduce the construction temperature; in order to solve the storage stabilizer and segregation problems, the grading of waste tire rubber powder is optimized, the particle fineness is specified, stabilizers are added, etc.; at the same time, the construction process is optimized to strive to obtain rubber asphalt with excellent performance. However, due to the characteristics of rubber asphalt materials themselves, if the "wet method" is used, the problems inherent in its production and construction cannot be completely solved. Summary of the invention
[0011] The invention provides a liquid rubber modifier / SBS composite modified asphalt and a preparation method thereof. Starting from the raw material of waste tire rubber powder, the properties thereof are changed so that the raw material can be effectively fused with base asphalt at a general construction temperature to form a new type of liquid rubber modified asphalt. Compared with the traditional method, the invention first converts the rubber powder into a liquid rubber asphalt modifier so that the raw material can fully react and swell with the base asphalt, thereby solving the problem of easy segregation. The mixing temperature of the liquid rubber asphalt modifier and the base asphalt is controlled at 160-170°C, thereby preventing the asphalt from being excessively aged due to high temperature. Meanwhile, the liquid rubber modifier has better compatibility with the asphalt, thereby improving the construction and workability.
[0012] To achieve the above object, the present invention provides a method for preparing a liquid rubber modifier / SBS composite modified asphalt, comprising the following steps:
[0013] S1. Preparation of liquid rubber modifier
[0014] S1-1, adding the pretreated waste tire rubber powder, cracking catalyst regeneration agent, oily adhesive and matrix asphalt into the rubber high-speed plasticizing unit according to the mass ratio of 100: (2-3.2): (20-30): 10;
[0015] S1-2, set the environmental conditions of the rubber high-speed plasticizing unit to 80°C, 800r / min high-speed stirring for 15min, add the liquid rubber modifier to the twin-screw extruder, the speed of the twin-screw extruder is 150r / min, and the liquid rubber modifier is subjected to mechanical shearing for 5min; the extrusion temperature of the twin-screw extruder is 230-290°C;
[0016] S1-3, sending the sheared liquid rubber modifier into a refiner for refining 20 times, outputting the formed liquid rubber modifier, and obtaining a finished liquid rubber modifier after cooling;
[0017] S2. Preparation of liquid rubber modifier / SBS composite modified asphalt
[0018] S2-1, heating the base asphalt and the liquid rubber modifier to 165°C respectively;
[0019] S2-2, the liquid rubber modifier, the matrix asphalt and the SBS were mixed in a mass ratio of (10-30):100:1, and stirred at a constant speed of 100 r / min for 20 min at 165°C to allow swelling;
[0020] S2-3. Keep the temperature of the liquid after swelling in step S2-2 at 165° C., and perform high-speed shearing in a shearing machine at a rotation speed of 7000 r / min for 30 minutes. After full fusion, obtain a liquid rubber modifier / SBS composite modified asphalt.
[0021] Preferably, the pretreatment in step S1-1 includes: placing the cracking catalyst regeneration agent in an environment of 50°C to 60°C for 12 hours for pretreatment, and placing the waste tire rubber powder, oily adhesive, and matrix asphalt in an environment of 40°C to 50°C for preheating for 4-6 hours.
[0022] Preferably, the fineness of the waste tire rubber powder is 60 mesh.
[0023] Preferably, the cracking catalyst regeneration agent includes 60% of a liquefaction cracking agent and 40% of a catalyst regeneration reducing agent, and the liquefaction cracking agent includes a rubber activator 420 and benzoic acid.
[0024] Preferably, the oily binder is a saponified oil.
[0025] Preferably, the base asphalt is one of SK-90#, Shell 90# and Caltex 90#.
[0026] Preferably, in step S1-1, the mass ratio of waste tire rubber powder, cracking catalyst regeneration agent, acidified oil and base asphalt is 100:2.6:30:10.
[0027] Preferably, in step S1-2, the extrusion temperature of the twin-screw extruder is 260°C.
[0028] Preferably, in step S2-2, the mass ratio of the liquid rubber modifier, the base asphalt and the SBS is 22:100:1.
[0029] The invention discloses a liquid rubber modifier / SBS composite modified asphalt and a preparation method thereof. The invention discloses a liquid rubber modifier / SBS composite modified asphalt and a preparation method thereof. Waste tire rubber powder is converted into a liquid rubber modifier so that the liquid rubber modifier can fully react and swell with matrix asphalt, thereby solving the problem of easy segregation. The mixing temperature of the liquid rubber asphalt modifier and the matrix asphalt is controlled at 160-170°C, thereby preventing the asphalt from being over-aged due to high temperature. Meanwhile, the liquid rubber modifier has better compatibility with asphalt, thereby improving construction and workability.
[0030] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a flow chart for the preparation of liquid rubber modifier;
[0032] Figure 2 The figure is a flow chart for the preparation of liquid rubber modified asphalt;
[0033] Figure 3 The test results of Mooney viscosity, crosslinking density and sol content of the liquid rubber modifier under various factor level conditions, where (a) is Mooney viscosity, (b) is crosslinking density, and (c) is sol content;
[0034] Figure 4 It is a statistical diagram of chemical bond breaking types during the devulcanization process of liquid rubber modifier;
[0035] Figure 5 The three major index test results of three types of base asphalts at different liquid rubber modifier dosages are shown in Figure 1. (a) is the 5°C ductility test result of three types of base asphalts at different liquid rubber modifier dosages; (b) is the softening point test result of three types of base asphalts at different liquid rubber modifier dosages; (c) is the 25°C needle penetration test result of three types of base asphalts at different liquid rubber modifier dosages.
[0036] Figure 6 The dynamic mechanical properties test results of different base asphalts and composite modified asphalts, where (a) is the complex modulus of different base asphalts and composite modified asphalts; (b) is the phase angle of different base asphalts and composite modified asphalts; (c) is the rutting factor of different base asphalts and composite modified asphalts;
[0037] Figure 7 The fluorescence microscope observation images of the asphalt modified by the liquid rubber modifier and the liquid rubber modifier / SBS composite modified asphalt in Example 4, wherein A is the fluorescence microscope observation image of the asphalt modified by the liquid rubber modifier, and B is the fluorescence microscope observation image of the liquid rubber modifier / SBS composite modified asphalt;
[0038] Figure 8 The SEM electron microscope scanning observation images of the base asphalt, liquid rubber modified asphalt, and liquid rubber modifier / SBS composite modified asphalt in Example 4, wherein A is the SEM electron microscope scanning observation image of the base asphalt, B is the SEM electron microscope scanning observation image of the liquid rubber modified asphalt, and C is the SEM electron microscope scanning observation image of the liquid rubber modifier / SBS composite modified asphalt;
[0039] Fig. 9 The temperature variation statistics of the base asphalt, the liquid rubber modifier modified asphalt and the liquid rubber modifier / SBS composite modified asphalt used in Example 4 are shown in FIG.
[0040] Fig.10 These are the infrared spectrum test results of the liquid rubber modifier sample, matrix asphalt sample, liquid rubber modified asphalt and liquid rubber modifier / SBS composite modified asphalt sample in Example 4, wherein A is the infrared spectrum of the liquid rubber modifier; B is the infrared spectrum of the matrix asphalt; C is the infrared spectrum of the liquid rubber modified asphalt; D is the infrared spectrum of the liquid rubber modifier / SBS composite modified asphalt. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical scheme and advantages disclosed in the embodiments of the present invention clearer, the embodiments of the present invention are further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the embodiments of the present invention and are not intended to limit the embodiments of the present invention. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application. Examples of the embodiments are shown in the accompanying drawings, where the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions.
[0042] It should be noted that the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or server that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or inherent to these processes, methods, products or devices.
[0043] Like reference numerals and letters denote similar items in the following drawings, and thus, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0044] Embodiment 1
[0045] Preparation of liquid rubber modifier, the process is as follows Figure 1 As shown, the specific steps include:
[0046] (1) The cracking catalyst regeneration agent is placed in an environment of 50°C to 60°C for 12 hours for pretreatment, and the waste tire rubber powder, oily adhesive, and matrix asphalt are placed in an environment of 40°C to 50°C for preheating for 4-6 hours.
[0047] Among them, the cracking catalyst regeneration agent includes a liquefaction cracking agent and a catalytic regeneration reducing agent, the liquefaction cracking agent includes a rubber activator 420 and benzoic acid, and the catalytic regeneration reducing agent is PTC-R (II) produced by Hebei Ruiwei Technology Co., Ltd.
[0048] The size of waste tire rubber powder is 60 mesh, and its physical and chemical technical indicators refer to the relevant requirements in "Road Waste Tire Rubber Powder" (JT / T 797-2019).
[0049] The oily adhesive is saponified oil.
[0050] The base asphalt includes one of SK-90#, Shell 90# and Caltex 90#.
[0051] (2) Add waste tire rubber powder, cracking catalyst regeneration agent, oily adhesive and base asphalt in a mass ratio of 100:(2-3.2):(20-30):10 into a rubber high-speed plasticizing unit.
[0052] (3) Start the rubber high-speed plasticizing unit, set the environmental condition to 80°C, and stir at 800 r / min for 15 minutes to achieve the regeneration, plasticization and liquefaction of the waste tire rubber powder.
[0053] (4) adding the incompletely liquefied liquid rubber modifier into a twin-screw extruder that has reached a set temperature, starting the twin-screw extruder at a speed of 150 r / min, and subjecting it to mechanical shearing for 5 minutes; the temperature of other zones of the twin-screw extruder is 180°C, and the extrusion temperature is 230-290°C.
[0054] (5) The sheared liquid rubber modifier is sent to a refiner and refined 20 times to output a formed liquid rubber modifier, which is then cooled to obtain a finished liquid rubber modifier.
[0055] The index values of liquid rubber modifier are shown in Table 1:
[0056] Table 1 Index values of liquid rubber modifiers
[0057] Technical indicators unit Index test value Index reference value Mooney viscosity ML(1+4)100℃ 25.1 ≤85 Crosslink density <![CDATA[10 -4 mol·cm -1 ]]> 0.93 ≤1.4 Sol content % 30.5 ≥20
[0058] Explore the effects of three factors and three levels on the Mooney viscosity, crosslinking density and sol content of the liquid rubber modifier, and determine the optimal ratio and extrusion temperature of the liquid rubber modifier. Among them, the three influencing factors and their test levels are shown in Table 2, and the orthogonal test scheme is shown in Table 3:
[0059] Table 2 Liquid rubber modifier test factors and levels
[0060]
[0061] Table 3 Orthogonal test scheme for liquid rubber modifier
[0062]
[0063]
[0064] The Mooney viscosity, crosslinking density and sol content of the liquid rubber modifier under each factor level condition were tested in turn, and the average values of the three indicators were calculated respectively. The orthogonal test test results are shown in Table 4 and Figure 3 As shown:
[0065] Table 4 Test results of Mooney viscosity, crosslinking density and sol content in orthogonal test group
[0066]
[0067]
[0068] Figure 3 (a) is the Mooney viscosity at different factor levels; analysis shows that each factor has a significant impact on the Mooney viscosity of the liquid rubber modifier, and the order of influence is: extrusion temperature > acidified oil dosage > cracking catalyst regeneration agent dosage. The increase in the dosage of cracking catalyst regeneration agent and acidified oil can reduce the Mooney viscosity of the liquid rubber modifier; as the extrusion temperature increases, the degree of rubber cracking increases, and the Mooney viscosity of the liquid rubber modifier decreases. The lower the Mooney viscosity of the liquid rubber modifier, the stronger its plasticity, the closer it is to the liquid state, and the better its working performance in modified asphalt.
[0069] (b) is the cross-linking density under different factor levels; analysis shows that the order of influence of various factors on the cross-linking density of liquid rubber modifier is: extrusion temperature > cracking catalyst regeneration agent dosage > acidified oil dosage, among which, the increase in the amount of acidified oil will slightly reduce the cross-linking density; when the amount of cracking catalyst regeneration agent increases to a certain extent, its catalytic effect will no longer increase, and the cross-linking density tends to be stable; the cross-linking density first decreases and then increases with the increase of extrusion temperature, mainly because the excessively high extrusion temperature not only breaks the cross-linking bonds, but also causes a large number of main chain breaks, resulting in a large number of small network structures, which increases the cross-linking density.
[0070] (c) Sol content at different factor levels; Analysis shows that the order of influence of various factors on the sol content of liquid rubber modifier is: extrusion temperature > cracking catalyst regeneration agent dosage > acidified oil dosage, among which the acidified oil dosage has a smaller effect on the sol content. With the increase of cracking catalyst regeneration agent dosage and extrusion temperature, the sol content increases significantly, indicating that increasing the catalyst dosage and raising the extrusion temperature can improve the desulfurization degree of waste tire rubber powder.
[0071] In summary, combined with the analysis of the influence of each factor level on each index of the liquid rubber modifier, it can be seen that the optimal process obtained after optimizing the Mooney viscosity, crosslinking density and sol content of the liquid rubber modifier is shown in Table 5.
[0072] Table 5 Results of orthogonal test optimal process analysis
[0073]
[0074] The main breakage of waste rubber during the desulfurization cracking process is the SS bond and SC bond. If the desulfurization conditions are not properly controlled, a large number of CC bonds will break, causing the rubber to degrade and lose its elastic properties. Therefore, the Horik theory is used to analyze the types of chemical bond breakage during the desulfurization process of liquid rubber modifiers under various preparation conditions. The results are as follows: Figure 4 shown.
[0075] Depend on Figure 4 Analysis shows that all index points are located between the two curves. The two points under A3 and C3 conditions are closer to the curve where only the main chain breaks than the points under other conditions, indicating that when the amount of cracking catalyst regeneration agent reaches 3.2% and the extrusion temperature reaches 290°C, the main chain breaks more during the desulfurization of rubber powder. Therefore, the amount of cracking catalyst regeneration agent and the extrusion temperature should not be too high. At the same time, under A1 and C1 conditions, the sol content is significantly lower than other conditions, indicating that the desulfurization effect is poor when the amount of cracking catalyst regeneration agent and the extrusion temperature are low.
[0076] In summary, combined with the preliminary results of each index and the main chain and cross-link bond breakage at different levels of each factor, the final preparation process of the liquid rubber modifier was determined to be A2B3C2, that is, the amount of cracking catalyst regeneration agent was 2.6%, the amount of acidified oil was 30%, and the extrusion temperature was 260 °C.
[0077] Embodiment 2
[0078] Preparation of liquid rubber modified asphalt, the process is as follows Figure 2 As shown, the specific steps include:
[0079] (1) Heat the base asphalt and liquid rubber modifier to about 165°C respectively.
[0080] (2) The liquid rubber modifier and the base asphalt are mixed in a ratio of (10-30):100, and stirred at a low speed (100 r / min) and a constant speed for 20 min at 165°C to allow swelling.
[0081] (3) The temperature of the liquid rubber modifier and the matrix asphalt was maintained at 165°C, and high-speed shearing was performed for 30 minutes in a shearing machine at a speed of 7000 r / min to achieve sufficient fusion.
[0082] (4) Output liquid rubber modified asphalt.
[0083] The liquid rubber modifier was added at 5 levels of 10%, 15%, 20%, 25% and 30%, and three base asphalts, SK-90#, Shell 90# and Caltex 90#, were used to make liquid rubber modified asphalt, and they were recorded as MA-SK90#, MA-Shell 90# and MA-Caltex 90#. The performance of the three preferred indicators of 5℃ elongation, softening point and 25℃ needle penetration of the three were tested to obtain the test results of various properties, and then the optimal dosage of the liquid rubber modifier was determined. The test results are shown in Table 6 and Figure 5 shown.
[0084] Table 6 Test results of three major indicators of three base asphalts at different liquid rubber modifier dosages
[0085]
[0086] Figure 5 (a) shows the 5°C ductility test results of three base asphalts at different liquid rubber modifier dosages. Analysis shows that as the liquid rubber modifier dosage increases, the ductility of the modified asphalt first increases and then tends to stabilize, indicating that when the liquid rubber modifier dosage increases to a certain extent, the influence on the low-temperature ductility of the modified asphalt decreases. The ductility increase of the modified asphalt with Shell 90# as the base asphalt is small, and the ductility change range is small with the change of the liquid rubber modifier dosage. Referring to the relevant requirements of the specification, it can be seen that only MA-SK90# can meet the requirements, and the liquid rubber modifier dosage is about 22%. If the optimal dosage of the liquid rubber modifier is determined according to the maximum ductility of each liquid rubber modified asphalt such as MA-SK90#, MA-Shell 90# and MA-Caltex 90#, it should be 22%, 15% and 22% respectively.
[0087] Figure 5(b) shows the softening point test results of three types of matrix asphalts at different liquid rubber modifier dosages. Analysis shows that the softening point of MA-SK90# increases with the increase of liquid rubber modifier dosage, and gradually stabilizes after exceeding 20% dosage, with only a slight increase. The softening point of MA-Shell 90# first increases slowly with the increase of liquid rubber modifier dosage, and increases rapidly after exceeding 13%, and then stabilizes after exceeding 20%. The softening point of MA-Caltex 90# increases rapidly with the increase of dosage, and decreases slowly after exceeding 22%.
[0088] According to the relevant requirements of the specification, it can be seen that MA-SK90# and MA-Shell 90# can meet the requirements, and the liquid rubber modifier dosage range should be 19-30% and 21-30% respectively. If the optimal softening point of each liquid rubber modified asphalt such as MA-SK90#, MA-Shell 90# and MA-Caltex 90# is determined, the optimal dosage of liquid rubber modifier should be 30%, 22% and 22% respectively.
[0089] Figure 5 (c) shows the 25°C penetration test results of three base asphalts at different liquid rubber modifier dosages. Analysis shows that the penetration of liquid rubber modified asphalt gradually decreases with the increase in liquid rubber modifier dosage, that is, the modified asphalt becomes harder. Referring to the relevant requirements of the specification, it can be seen that MA-SK90#, MA-Shell 90# and MA-Caltex 90# can all meet the requirements, and the liquid rubber modifier dosage range should be 18-30%, 23-30% and 13-30% respectively. In the hot southern regions, asphalt with low penetration is suitable, and roads with large traffic volume are also suitable for asphalt with low penetration, so it is necessary to choose according to the actual situation.
[0090] Embodiment 3
[0091] SBS is further introduced into the liquid rubber modified asphalt to form a liquid rubber modifier / SBS composite modified asphalt. The liquid rubber modifier / SBS composite modified asphalt is prepared by simultaneously adding SBS and liquid rubber to the base asphalt and shearing at high speed during the preparation process of the liquid rubber modified asphalt in Example 2, with the temperature and shear parameters unchanged, and the SBS content being 1%.
[0092] Based on the changes in the three major indicators of the above three modified asphalts, the indicators of MA-SK90# are relatively good, and the performance is better when the liquid rubber modifier is added at about 20%. Therefore, SK90# can be initially selected as the base asphalt, and the three major indicators of liquid rubber modifier / SBS composite modified asphalt can be compared when the liquid rubber modifier is added at 20%. Finally, the comparison of the test results of the three major indicators of MA-SK90# and liquid rubber modifier / SBS composite modified asphalt is shown in Table 7.
[0093] Table 7 Comparison of performance indicators of MA-SK90# and liquid rubber modifier / SBS composite modified asphalt
[0094]
[0095] From the analysis in Table 7, it can be seen that the softening point and 5°C ductility of the liquid rubber modifier / SBS composite modified asphalt are significantly improved compared with MA-SK90#. Among them, the 5°C ductility is improved by 64%, indicating that SBS can form a good physical cross-linking network in the asphalt when it is modified in conjunction with the liquid rubber modifier, thereby improving the ductility of the asphalt.
[0096] The softening point of liquid rubber modifier / SBS composite modified asphalt is 10℃ higher than that of MA-SK90#, indicating that the high temperature performance of liquid rubber modifier / SBS composite modified asphalt is better; there is little difference between the two in terms of needle penetration. At the same time, both can meet the requirements of the specification well.
[0097] In general, the introduction of SBS significantly improved the penetration and ductility of liquid rubber modified asphalt, indicating that liquid rubber modifier / SBS composite modified asphalt is more suitable for promotion and application in the engineering field.
[0098] Embodiment 4
[0099] A method for preparing a liquid rubber modifier / SBS composite modified asphalt comprises the following steps:
[0100] (1) The cracking catalyst regeneration agent was placed in an environment of 50°C for 12 hours for pretreatment, and 60-mesh waste tire rubber powder, oily adhesive, and SK-90# were placed in an environment of 50°C for 5 hours for preheating.
[0101] The cracking catalyst regeneration agent includes rubber activator 420 and benzoic acid.
[0102] The oily adhesive is saponified oil, which consists of 10.7% palmitic acid, 21.5% oleic acid, 29.2% linoleic acid, 6.5% heptadecane, 4.8% 8-heptadecene, 2.1% (1-methyldecyl) benzene, and 25.2% other components.
[0103] (2) Add waste tire rubber powder, cracking catalyst regeneration agent, acidified oil and base asphalt in a mass ratio of 100:2.6:30:10 into a rubber high-speed plasticizing unit.
[0104] (3) Start the rubber high-speed plasticizing unit, set the environmental condition to 80°C, and stir at 800r / min for 15min to achieve the regeneration, plasticization and liquefaction of the waste tire rubber powder;
[0105] (4) Add the incompletely liquefied liquid rubber modifier to the twin-screw extruder that has reached the set temperature, start the twin-screw extruder at a speed of 150 r / min, and perform mechanical shearing for 5 minutes; the temperature of other zones of the twin-screw extruder is 180°C, and the extrusion temperature is 260°C.
[0106] (5) The sheared liquid rubber modifier is sent to a refiner and refined 20 times to output a formed liquid rubber modifier, which is then cooled to obtain a finished liquid rubber modifier.
[0107] (6) Heat the base asphalt and liquid rubber modifier to 165°C respectively.
[0108] (7) The liquid rubber modifier and the base asphalt were mixed in a ratio of 22:100, and high-speed shearing was performed for 30 minutes in a shearing machine at a rotation speed of 7000 r / min to achieve sufficient fusion, and the liquid rubber modifier modified asphalt was output, which was recorded as MA-SK90#.
[0109] (8) The liquid rubber modifier, base asphalt and SBS were mixed in a mass ratio of 22:100:1, and high-speed shearing was carried out for 30 minutes in a shearing machine at a rotation speed of 7000 r / min to achieve sufficient fusion, and a liquid rubber modifier / SBS composite modified asphalt was output, which was recorded as MAS-SK90#.
[0110] Embodiment 5
[0111] A method for preparing a liquid rubber modifier / SBS composite modified asphalt is the same as that of Example 4, except that:
[0112] The base asphalt used is Shell 90#, the prepared liquid rubber modifier modified asphalt is recorded as MA-Shell 90#; the liquid rubber modifier / SBS composite modified asphalt is recorded as MAS-Shell 90#.
[0113] Embodiment 6
[0114] A method for preparing a liquid rubber modifier / SBS composite modified asphalt is the same as that of Example 4, except that:
[0115] The base asphalt used is Caltex 90#, the prepared liquid rubber modifier modified asphalt is recorded as MA-Caltex 90#; the liquid rubber modifier / SBS composite modified asphalt is recorded as MAS-Caltex 90#.
[0116] Experimental Test 1
[0117] In order to accurately evaluate the road performance of modified asphalt, the rheological properties of asphalt should be considered from the perspective of dynamic mechanical properties: the dynamic shear rheology test (DSR) is used to test the high-temperature rheological properties of the three base asphalts SK90#, Shell 90# and Caltex 90# in the above-mentioned embodiments four to six, and the three liquid rubber modifiers / SBS composite modified asphalts MAS-SK90#, MAS-Shell 90# and MAS-Caltex 90#, respectively, to obtain the complex shear modulus G*, phase angle δ, and rutting factor G* / sinδ and other parameters of the three asphalts. The dynamic shear rheometer used in the test is the discovery series produced by TA, which adopts the strain control mode. The test temperatures were set to 46°C, 52°C, 58°C, 64°C, 70°C, and 76°C, respectively. The final test results are as follows. Figure 6 shown.
[0118] Figure 6 (a) is the complex modulus G*. Analysis shows that the complex modulus of different base asphalts and composite modified asphalts gradually decreases with increasing temperature and eventually tends to the same level range. At the same temperature, the G* of different types of liquid rubber modifiers / SBS composite modified asphalts is significantly higher than that of base asphalt, which shows that the incorporation of liquid rubber can be evenly dispersed in the asphalt phase, improving the stiffness modulus of asphalt and increasing its ability to resist deformation. At the same time, comparing different liquid rubber modifiers / SBS composite modified asphalt G*, MAS-SK90# shows better resistance to deformation than MAS-Shell 90# and MAS-Caltex 90#.
[0119] Figure 6 (b) is the phase angle δ. Analysis shows that the δ values of different base asphalts and composite modified asphalts increase with increasing temperature. The δ value of liquid rubber modifier / SBS composite modified asphalt is significantly lower than that of base asphalt, showing stronger elasticity. This is because the liquid rubber molecules and the molecules in the asphalt are interlocked and cross-linked to form a cross-linked network, which increases the rigidity of the modified asphalt system, hinders flow deformation, and reduces the viscosity. The increase in the δ value of liquid rubber modifier / SBS composite modified asphalt with increasing temperature is slightly greater than that of base asphalt, indicating that the liquid rubber modifier / SBS composite modified asphalt has more viscoelastic conversion components and unstable performance, which is consistent with the segregation characteristics of the liquid rubber modifier. Compared with the three composite modified asphalts, MAS-SK90# has a smaller δ value and better elastic performance, but the three tend to be consistent when the temperature is greater than 70°C.
[0120] Figure 6(c) is the rutting factor G* / sinδ. Analysis shows that the rutting factor of the liquid rubber modifier / SBS composite modified asphalt is significantly higher than that of the base asphalt, indicating that the liquid rubber modifier and SBS can greatly improve the anti-rutting performance of asphalt. Comparing the rutting factors of various modified asphalts, MAS-SK90# is relatively high and has better anti-rutting performance. The anti-rutting factors of the three modified asphalts are ranked as follows: MAS-SK90#>MAS-Caltex 90#>MAS-Shell 90#. Combined with the relationship between the anti-rutting performance of different base asphalts, although the difference in the rutting factors of different base asphalts is small, it is not difficult to find that the order of the rutting factors of the modified asphalt is consistent with that of its base asphalt, and the anti-rutting performance of the liquid rubber modified asphalt is related to the performance of its base asphalt.
[0121] Experimental Test 2
[0122] The base asphalt, liquid rubber modifier, liquid rubber modifier modified asphalt, and liquid rubber modifier / SBS composite modified asphalt used in Examples 4 to 6 were tested and analyzed. The main tests conducted included fluorescence microscopy observation test, SEM electron microscopy observation test, differential scanning calorimetry test, and infrared spectroscopy test.
[0123] 1. Fluorescence microscopy observation and analysis
[0124] ① Place the asphalt sample in an oven and heat it to a fluid state for later use. Use a clean glass rod to dip a small amount of asphalt and quickly drop it on the prepared clean slide. While it is still hot, evenly distribute it into a thin layer and cover it with a cover glass for subsequent tests.
[0125] ② Turn on the fluorescence microscope, fix the test sample, adjust various parameters to collect the asphalt microscopic phase structure image, and save it to the computer.
[0126] The liquid rubber modifier modified asphalt and the liquid rubber modifier / SBS composite modified asphalt in Example 4 were observed under a fluorescence microscope, and the test results were as follows: Figure 7 As shown in A and B. Analysis shows that:
[0127] (1) After desulfurization and activation, the liquid rubber modifier is evenly dispersed in the matrix asphalt, indicating that it is highly compatible with asphalt, but there are still some agglomerated spots, indicating that even at higher temperatures and under longer shearing time, the liquid rubber is not completely compatible with asphalt. The main reason may be that the liquid rubber modifier swells in the asphalt after desulfurization, and most of the main chains of the liquid rubber modifier are stretched and opened, while the main chains of a few liquid rubber molecules are more entangled, which makes most of the liquid rubber molecules compatible with asphalt, while a few of them have agglomerated spots.
[0128] (2) The liquid rubber modifier / SBS compound is in a mixed state with asphalt. At a certain temperature and shear rate, the liquid rubber modifier / SBS compound molecules are connected with the asphalt molecules to form a spatial grid structure. The molecules cross each other and form a relatively stable sol-gel structure system. The main chain of the liquid rubber modifier is completely opened, and the swelling and compatibility are relatively large. Therefore, it can be seen that the modification effect of the liquid rubber modifier / SBS compound on the base asphalt may be better than that of the simple liquid rubber modified asphalt.
[0129] (II) SEM electron microscope observation test and analysis
[0130] A German Zeiss tungsten filament scanning electron microscope (EVO MA10) was used to perform SEM scanning observation on the three samples of the base asphalt, liquid rubber modified asphalt, and liquid rubber modifier / SBS composite modified asphalt prepared in Example 4.
[0131] Before observation, in view of the insulating properties of asphalt samples, in order to enable the sample surface to emit secondary electrons, a layer of heavy metal particles needs to be sprayed on the sample surface. Heavy metals can emit secondary electron signals under the bombardment of electron beams. This test uses the vacuum coating method, that is, a layer of metal powder with a thickness of 20mm is coated on the surface of the asphalt sample in a vacuum, and then the gold-plated sample is placed in the electron microscope sample chamber for observation. The test instrument display and the scanning test results of each sample are shown in the figure below. Figure 8 As shown in A, B, and C.
[0132] Analysis shows that when no modifier is added, the base asphalt presents a uniform continuous phase, and the surface is approximately "smooth"; after the addition of liquid rubber, the liquid rubber molecules absorb the light components of the base asphalt, swelling occurs, and they are well compatible with asphalt, with basically no signs of cracks on the surface, and they may have undergone certain chemical cross-linking with asphalt, resulting in a richer microscopic morphology of the mixture, or a tendency to form a network structure, and then the "wrinkle" phenomenon appears; after the addition of liquid rubber modifier / SBS composite, the liquid rubber modifier / SBS modified asphalt forms a more sufficient network structure, with a richer microscopic morphology, and the macroscopic manifestation is that the viscosity, ductility and PG high-temperature grade of the modified asphalt are significantly increased, and the low-temperature crack resistance and high-temperature stability are improved.
[0133] (III) Differential scanning calorimetry test and analysis
[0134] A diomond DSC power compensation differential scanning calorimeter was used, with a temperature rise rate of 10°C / min, a nitrogen atmosphere, a nitrogen flow rate of 50 mL / min, a starting temperature of 30°C, and an ending temperature of 210°C. The DSC instrument was used to measure the base asphalt, the liquid rubber modifier modified asphalt, and the liquid rubber modifier / SBS composite modified asphalt used in Example 4, respectively. The results are shown in FIG. Fig. 9 shown.
[0135] It can be seen that the DSC curves of the three asphalts have basically the same trend. But in general, the DSC curve of the liquid rubber modifier / SBS composite modified asphalt has the smallest displacement from the baseline, followed by the liquid rubber modified asphalt. This shows that the rate at which the liquid rubber modifier / SBS composite modified asphalt absorbs or releases heat is slower than that of the liquid rubber modified asphalt; and the rate at which the liquid rubber modified asphalt absorbs or releases heat is slower than that of the base asphalt.
[0136] Therefore, thermal stability: liquid rubber modifier / SBS composite modified asphalt> liquid rubber modified asphalt> base asphalt. Rubber / SBS composite modified asphalt and liquid rubber modified asphalt did not show absorption peaks after the temperature exceeded 170°C, which shows that after reaching a certain temperature, the aggregation state of the two modified asphalt components has basically changed and is in a viscous flow state. At the same time, it also shows that the added liquid rubber modifier and chemical SBS modifier absorb a certain amount of light components in the asphalt, increasing the proportion of asphaltene and colloid, thereby reducing the temperature sensitivity of the asphalt. Therefore, this well explains the phenomenon of the increase in softening point after the addition of liquid rubber modifier and chemical SBS modifier to the base asphalt. The changes and differences in the DSC curves of these three asphalts further illustrate the influence of chemical SBS modifier on the liquid rubber and asphalt blending system. It is necessary to add a certain amount of SBS to the liquid rubber modified asphalt.
[0137] (IV) Infrared spectrum test and analysis
[0138] The infrared spectrometer used is the FIIR-8400S Fourier transform infrared spectrometer produced by Shimadzu Corporation of Japan, with a resolution of 0.1 to 0.005 cm -1 , scanning times 32 times, test range 4000cm -1 . The potassium bromide tablet method was used for analysis and determination. 300 mg of potassium bromide and 2 mg of solid sample were ground into micron-grade fine powder, pressed into transparent sheets by a hydraulic press at a pressure of 5 to 10 MPa in a mold, and then placed under the light path for analysis. Potassium bromide was selected as an analytical reagent. The moisture in potassium bromide was driven off by drying in an oven at 150 to 200°C for 6 hours, and then placed in a dryer for cooling. Special attention should be paid to the fact that the entire process should be carried out in a dry environment.
[0139] The liquid rubber modifier sample, the matrix asphalt sample, the liquid rubber modified asphalt and the liquid rubber modifier / SBS composite modified asphalt sample in Example 4 were subjected to infrared spectroscopy tests. After being processed by the data software, the test results are as follows: Fig.10 As shown in A, B, C, and D.
[0140] Fig.10 A is the infrared spectrum of liquid rubber modifier; the liquid rubber modifier has a wavelength of 2600-3000 cm -1 In the range of 2.5 ℃ and 1.5 ℃, the infrared spectrum of liquid rubber modifier shows strong absorption peaks, among which -CH2 has the largest absorption. These absorption peaks are cycloalkanes and alkanes -CH (alkanes: -CH stretching vibration 2850~3000cm -1 ) stretching vibration results. 1600cm -1 The nearby peaks are partly caused by the conjugated double bond C=C (benzene ring skeleton vibration) and partly by C=O absorption. In the fingerprint region 600-900cm -1 In the wavenumber range, the absorption peak that appears is caused by the out-of-plane swinging vibration of -CH on the benzene ring.
[0141] Fig.10 B is the infrared spectrum of the matrix asphalt; the matrix asphalt has a wave number of 2500-3000cm -1 In the range of 2800-3000 cm-1, the infrared spectrum of the matrix asphalt shows strong absorption peaks, which should be caused by the stretching vibration of cycloalkanes and alkanes -CH (alkanes: -CH stretching vibration 2850-3000 cm-1 -1 ) stretching vibration, among which -CH2 has the largest absorption peak. The wave number range is 1450~1600cm -1 The absorption peak should be caused by the conjugated double bond C=C (benzene ring skeleton vibration); the wave number range is 1340~1450cm -1 The absorption peak should be caused by -CH bending vibration; the wave number is between 1000 and 1300 cm -1 The absorption peak is the result of CO stretching vibration; the wave number range is 680~880cm -1 The absorption peak is the result of the out-of-plane bending vibration of -CH.
[0142] By comparison Fig.10 Middle A and Fig.10 B can analyze the changes in functional groups and molecular structures before and after the addition of liquid rubber modifiers to asphalt. If there is only physical interaction between the liquid rubber and the matrix asphalt, and no chemical interaction, the absorption peak in the infrared spectrum of the liquid rubber modified asphalt should be a simple geometric superposition of the absorption peaks of the liquid rubber and the matrix asphalt, and the position of the absorption peak should be the same, but the intensity will change.
[0143] Fig.10C is the infrared spectrum of liquid rubber modified asphalt; at wave number 2500~3000cm -1 A strong absorption peak appeared in the range, and the position of the absorption peak was very similar to that of the matrix asphalt, with a slight change in intensity, which was caused by the addition of liquid rubber modifier.
[0144] In addition, comparison Fig.10 Medium B and Fig.10 It can be found in C that the infrared spectrum of the matrix asphalt has a wave number of 750cm -1 The absorption peaks around Fig.10 The peak in C disappeared, while the liquid rubber modifier had an absorption peak at the corresponding position. It can be inferred that a chemical reaction occurred between the functional groups of the matrix asphalt and the active substances in the liquid rubber modifier.
[0145] Fig.10 D in the figure is the infrared spectrum of liquid rubber modifier / SBS composite modified asphalt; Fig.10 Middle C and Fig.10 It can be found in Figure D that the positions of the infrared spectra absorption peaks of the two are basically the same, but the size of the absorption peaks is different, and no new absorption peaks appear. However, after adding the chemical SBS modifier, the several absorption peaks of the infrared spectrum of the liquid rubber modified asphalt are weakened to varying degrees. This is because the added chemical SBS modifier greatly increases the activity of the liquid rubber modifier, promotes the physical compatibility and swelling between the liquid rubber modifier and the matrix asphalt, and is conducive to accelerating and improving the formation of a network structure between the two.
[0146] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a liquid rubber modifier / SBS composite modified asphalt, characterized in that: The steps include: S1. Preparation of liquid rubber modifier S1-1, adding the pretreated waste tire rubber powder, cracking catalyst regeneration agent, oily adhesive and matrix asphalt into the rubber high-speed plasticizing unit according to the mass ratio of 100: (2-3.2): (20-30): 10; S1-2, set the environmental conditions of the rubber high-speed plasticizing unit to 80°C, 800r / min high-speed stirring for 15min, add the liquid rubber modifier to the twin-screw extruder, the speed of the twin-screw extruder is 150r / min, and the liquid rubber modifier is subjected to mechanical shearing for 5min; the extrusion temperature of the twin-screw extruder is 230-290°C; S1-3, sending the sheared liquid rubber modifier into a refiner for refining 20 times, outputting the formed liquid rubber modifier, and obtaining a finished liquid rubber modifier after cooling; S2. Preparation of liquid rubber modifier / SBS composite modified asphalt S2-1, heating the base asphalt and the liquid rubber modifier to 165°C respectively; S2-2, the liquid rubber modifier, the matrix asphalt and the SBS were mixed in a mass ratio of (10-30) : 100 : 1, and stirred at a constant speed of 100 r / min for 20 min at 165°C to allow swelling; S2-3. Keep the temperature of the liquid after swelling in step S2-2 at 165° C., and perform high-speed shearing in a shearing machine at a rotation speed of 7000 r / min for 30 minutes. After full fusion, obtain a liquid rubber modifier / SBS composite modified asphalt.
2. The method for preparing a liquid rubber modifier / SBS composite modified asphalt according to claim 1, characterized in that: The pretreatment in step S1-1 includes: placing the cracking catalyst regeneration agent in an environment of 50°C to 60°C for 12 hours for pretreatment, and placing the waste tire rubber powder, oily adhesive, and matrix asphalt in an environment of 40°C to 50°C for preheating for 4-6 hours.
3. The method for preparing a liquid rubber modifier / SBS composite modified asphalt according to claim 1, characterized in that: The fineness of waste tire rubber powder is 60 mesh.
4. The method for preparing a liquid rubber modifier / SBS composite modified asphalt according to claim 1, characterized in that: The cracking catalyst regeneration agent includes a liquefaction cracking agent and a catalyst regeneration reducing agent, and the liquefaction cracking agent includes a rubber activator 420 and benzoic acid.
5. The method for preparing a liquid rubber modifier / SBS composite modified asphalt according to claim 1, characterized in that: The oily adhesive is saponified oil.
6. The method for preparing a liquid rubber modifier / SBS composite modified asphalt according to claim 1, characterized in that: The base asphalt is one of SK-90#, Shell 90# and Caltex 90#.
7. The method for preparing a liquid rubber modifier / SBS composite modified asphalt according to claim 1, characterized in that: In step S1-1, the mass ratio of waste tire rubber powder, cracking catalyst regeneration agent, acidified oil and base asphalt is 100:2.6:30:
10.
8. The method for preparing a liquid rubber modifier / SBS composite modified asphalt according to claim 1, characterized in that: In step S1-2, the extrusion temperature of the twin-screw extruder is 260°C.
9. The method for preparing a liquid rubber modifier / SBS composite modified asphalt according to claim 1, characterized in that: In step S2-2, the mass ratio of the liquid rubber modifier, the base asphalt, and the SBS is 22:100:
1.
10. A liquid rubber modifier / SBS composite modified asphalt prepared by the method for preparing a liquid rubber modifier / SBS composite modified asphalt as claimed in any one of claims 1 to 9.