Asphalt preparation process for middle-high voltage power cable

Through demulsification treatment and temperature control technology, combined with the use of inert gas media, the problems of poor coking and viscosity in asphalt preparation are solved, and the fluidity and laying effect of asphalt are improved.

CN118931215APending Publication Date: 2024-11-12ZHEJIANG ZHONGDA CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172300.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When the existing asphalt preparation process uses water and thermally conductive oil to heat it repeatedly, the asphalt is prone to coking, resulting in poor viscosity and affecting laying and use.

Method used

Using demulsification treatment and temperature control technology, through the fixed ratio design of the emulsifier aqueous solution to asphalt, crushing equipment is used to form a uniform and fine particle asphalt emulsion, and use inert gas as a medium when heating to avoid temperature loss and coking and improve flow sex.

Benefits of technology

Ensure the flowability and quality of asphalt, avoid coking, and improve the overall solidification effect of medium and high voltage power cable laying.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931215A_ABST
    Figure CN118931215A_ABST
Patent Text Reader

Abstract

The invention discloses an asphalt preparation process for a middle-high voltage power cable. The asphalt preparation process comprises the following steps: S1, raw material preparation stage: selecting asphalt, water, an emulsifier, acid and a modifier; s2, a raw material pretreatment stage, wherein the asphalt selected in the S1 stage is subjected to demulsification treatment; s3, a liquid soap preparation stage: selecting a proper emulsifier and an additive to prepare an emulsifier aqueous solution according to the emulsified asphalt obtained in the S2 stage; s4, a temperature control stage: respectively controlling the temperatures during preparation in S1, S2 and S3; and S5, a constant proportion stage: a tester samples the demulsified asphalt obtained in the step S2 and the emulsifier aqueous solution obtained in the step S2 for constant proportion, and a proper production proportion is obtained. According to the asphalt preparation process for the middle-high voltage power cable, demulsification treatment is performed on asphalt in different modes in the step S2, so that the asphalt preparation process is suitable for different processing environments during asphalt preparation, limitation during asphalt preparation is reduced, and an emulsifier aqueous solution with a proper proportion is conveniently prepared according to the quality of emulsified asphalt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of asphalt preparation, and specifically to an asphalt preparation process for medium and high voltage power cables. Background Art

[0002] In the production process of 110KV and above high-voltage power cables, the anti-corrosion coating process of the metal sheath is an important process. Generally, the asphalt anti-corrosion layer is applied before the sheath unit enters the head for extrusion. At present, most domestic high-voltage cable manufacturers use heated cable asphalt. After searching, it is found that the asphalt preparation method in the prior art is typical, such as the invention of publication number CN201910808698.2, which belongs to the field of asphalt preparation process. Specifically, it is a road asphalt preparation process. The reaction device used in the preparation process includes a controller, a shell and a heating sleeve; the controller is used to control the normal operation of the reaction device; the end cover is provided with a feeding port and a motor; the feeding port is symmetrically arranged on the end cover; the motor is fixed to the end cover, and a transmission unit and a cleaning unit are provided inside the shell; the transmission unit includes a No. 1 shaft, a gear belt and a screw; the cleaning unit includes an isolation plate, a push rod and a cleaning plate; the heating sleeve is sleeved on the bottom of the shell to heat and insulate the mixture inside the shell; the transmission unit and the cleaning unit are coordinated to achieve full reaction between the mixture and the cleaning of the isolation plate surface by the cleaning plate, thereby improving the stirring and reaction efficiency.

[0003] In summary, when the existing asphalt preparation process uses water heating and heat transfer oil heating multiple times, the asphalt on the inner wall of the heating equipment will coke due to the temperature heating. At the same time, the asphalt is viscous and has poor fluidity, which will affect the paving and use of asphalt. In view of the above problems, the existing equipment needs to be improved. Summary of the invention

[0004] The purpose of the present invention is to provide an asphalt preparation process for medium and high voltage power cables to solve the problem that in the existing asphalt preparation process proposed in the above background technology, when water heating and heat transfer oil heating are used multiple times, the asphalt on the inner wall of the heating equipment will coke due to temperature heating, and the asphalt is viscous and has poor fluidity, which will affect the laying and use of the asphalt.

[0005] To achieve the above object, the present invention provides the following technical solution: a process for preparing asphalt for medium and high voltage power cables, comprising:

[0006] S1: Raw material preparation stage:

[0007] Select asphalt, water, emulsifier, acid and modifier;

[0008] S2: Raw material pretreatment stage:

[0009] The asphalt selected in the S1 stage is subjected to demulsification treatment;

[0010] S3: Soap preparation stage:

[0011] According to the emulsified asphalt obtained in the S2 stage, a suitable emulsifier and additives are selected to prepare an emulsifier aqueous solution;

[0012] S4: Temperature control stage:

[0013] The temperatures during the preparation of S1, S2 and S3 are controlled separately;

[0014] S5: Fixed ratio stage:

[0015] The test personnel sampled and determined the ratio of the demulsified asphalt obtained from S2 and the emulsifier aqueous solution obtained from S2 to obtain the appropriate production ratio;

[0016] S6: Emulsification of asphalt:

[0017] After the S5 ratio is reached, the asphalt and the emulsifier aqueous solution are put into the crushing equipment together. After the mechanical action of the crushing equipment such as pressurization, shearing, grinding, etc., the asphalt is formed into uniform and fine particles, which are stably and evenly dispersed in the soap solution to form an oil-in-water asphalt emulsion.

[0018] S7: Storage of emulsified bitumen:

[0019] Emulsified asphalt passes through the cooling device and enters the storage tank;

[0020] S8: Asphalt paving use:

[0021] The asphalt stored in S8 is paved using inert gas as the medium during transportation.

[0022] Preferably, the asphalt selected in the S1 stage accounts for 30%-60% of the total mass of the emulsified asphalt, and the asphalt temperature is relatively hot to 120°C-140°C.

[0023] Preferably, the demulsification treatment of asphalt in the S2 stage adopts two methods: Method 1, by slowly heating with a low fire, the asphalt is prevented from aging and deteriorating due to high temperature. In the absence of a thermometer, the temperature can be judged to be appropriate by observing whether the surface of the liquid is shiny, no longer bubbling, and whether there is blue smoke, so as to obtain the asphalt after liquid demulsification; Method 2, the liquid asphalt can also be stirred with solvents such as diesel and kerosene, or emulsified with water using an emulsifier to obtain emulsified asphalt.

[0024] Preferably, the temperature of the emulsifier aqueous solution obtained in the S3 stage is maintained at 55° C.-75° C. before entering the equipment.

[0025] Preferably, the temperature control in S4 adopts water heating and heat transfer oil heating, and both water heating and heat transfer oil heating use inert gas as the medium to heat the asphalt.

[0026] Preferably, the particle size of the particles obtained by the crushing equipment in S6 is 0.1 to 5 microns, and the crushing equipment used in S6 is an emulsifier.

[0027] Preferably, the cooling device used for the emulsified asphalt in S7 is circulating water cooling and dry ice cooling, and the storage pipe used in S7 has a built-in stirring device, and the stirring device uses timed stirring.

[0028] Preferably, the temperature of the inert gas in S8 is 300° C.-400° C., and both the water heating and the heat transfer oil heating use the inert gas as the medium to heat the asphalt.

[0029] Preferably, the ratio of the S8 inert gas to asphalt is 30:70, and the temperature of the inert gas introduced during the water heating is 300°C-400°C.

[0030] Preferably, the temperature of the inert gas introduced during the thermal oil heating is 310°C-350°C.

[0031] Compared with the prior art, the invention has the following beneficial effects: the asphalt preparation process for medium and high voltage power cables,

[0032] The present invention is suitable for different processing environments during asphalt preparation through different demulsification treatments of asphalt in S2, reduces limitations during asphalt preparation, and facilitates the preparation of an appropriate proportion of an emulsifier aqueous solution according to the quality of the emulsified asphalt. The independent temperature control design of S2 and S3 facilitates targeted heating according to the type of raw materials heated by the asphalt, avoids temperature runaway during heating, ensures that the temperature is accurately controlled, and avoids affecting the quality of asphalt preparation. The design of S5 facilitates accurate control of the optimal ratio between the emulsified asphalt and the emulsifier aqueous solution, which is conducive to conducting experiments in advance to obtain finished products and avoids subsequent large-scale asphalt preparation mixing. When the quality is poor, the emulsified asphalt is cooled by circulating water cooling and dry ice cooling in S6, which makes it easy to cool the asphalt quickly in a short time. At the same time, it can also protect the outside of the asphalt preparation device to reduce safety hazards. In addition, when heating and transporting using the temperature of S2 and S3, inert gas is used as a protective layer or driving force to form a protective layer on the inner wall of the heating device of S2 and S3 to avoid coking of the outer layer of asphalt and the heating device. At the same time, it can also increase the flow rate of asphalt with a certain viscosity to avoid local condensation when laying medium and high voltage power cables, affecting the overall solidification effect during laying. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a schematic diagram of the preparation process of the present invention;

[0034] Figure 2 This is a comparison chart of the extension values ​​of the present invention;

[0035] Figure 3 This is a comparison chart of the softening degree of the present invention;

[0036] Figure 4 This is a flow velocity comparison chart of the present invention. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] See also Figure 1-4 The present invention provides a technical solution: a process for preparing asphalt for medium and high voltage power cables.

[0039] Embodiment 1

[0040] S1: Raw material preparation stage:

[0041] Select asphalt, water, emulsifier, acid and modifier;

[0042] The asphalt selected in the S1 stage accounts for 30%-60% of the total mass of the emulsified asphalt, and the asphalt temperature is heated to 120℃-140℃.

[0043] S2: Raw material pretreatment stage:

[0044] The asphalt selected in the S1 stage is subjected to demulsification treatment;

[0045] There are two methods for demulsifying asphalt in the S2 stage: Method 1: slowly heat the asphalt over a low fire to prevent it from aging and deteriorating due to high temperature. In the absence of a thermometer, the temperature can be judged to be appropriate by observing whether the liquid surface is shiny, no longer bubbling, and whether there is blue smoke coming out, so as to obtain the asphalt after liquid demulsification. Method 2: liquid asphalt can also be stirred with solvents such as diesel and kerosene, or emulsified with water using an emulsifier to obtain emulsified asphalt. The different demulsification methods of asphalt in S2 are suitable for different processing environments during asphalt preparation, reduce the limitations during asphalt preparation, and facilitate the preparation of an appropriate proportion of emulsifier aqueous solution according to the quality of the emulsified asphalt.

[0046] S3: Soap preparation stage:

[0047] According to the emulsified asphalt obtained in the S2 stage, a suitable emulsifier and additives are selected to prepare an emulsifier aqueous solution;

[0048] The temperature of the emulsifier aqueous solution obtained in the S3 stage is maintained at 55℃-75℃ before entering the equipment. The independent temperature control design of S2 and S3 facilitates targeted heating according to the type of raw materials for asphalt heating, avoids temperature runaway during heating, ensures accurate temperature control, and avoids affecting the quality of asphalt preparation.

[0049] S4: Temperature control stage:

[0050] The temperatures during the preparation of S1, S2 and S3 are controlled separately;

[0051] Temperature control in S4 uses water heating and thermal oil heating;

[0052] The temperature of the inert gas introduced during the heating of the heat transfer oil is 310℃-350℃. When the temperature of S2 and S3 is used for heating and transportation, the inert gas is used as a protective layer or driving force to form a protective layer on the inner wall of the heating device of S2 and S3 to avoid coking of the outer asphalt and the heating device. At the same time, it can also increase the flow rate of asphalt with a certain viscosity to avoid local condensation when laying medium and high voltage power cables, affecting the overall solidification effect during laying.

[0053] S5: Fixed ratio stage:

[0054] The test personnel sampled and determined the ratio of the demulsified asphalt obtained by S2 and the emulsifier aqueous solution obtained by S2 to obtain the appropriate production ratio. Through the design of S5, it is convenient to accurately control the optimal ratio between the emulsified asphalt and the emulsifier aqueous solution, which is conducive to conducting tests in advance to obtain the finished product and avoid poor quality in subsequent large-scale asphalt preparation and mixing;

[0055] The particle size of S6 obtained by the crushing equipment is 0.3 to 6 microns, and the crushing equipment used in S6 is an emulsifier, so that the crushed particles can be more fully dispersed in the emulsifier aqueous solution.

[0056] S6: Emulsification of asphalt:

[0057] After the S5 ratio is reached, the asphalt and the emulsifier aqueous solution are put into the crushing equipment together. After the mechanical effects of the crushing equipment such as pressurization, shearing, and grinding, the asphalt is formed into uniform and fine particles, which are stably and evenly dispersed in the soap solution to form an oil-in-water asphalt emulsion.

[0058] S7: Storage of emulsified bitumen:

[0059] Emulsified asphalt passes through the cooling device and enters the storage tank.

[0060] Embodiment 2

[0061] S1: Raw material preparation stage:

[0062] Select asphalt, water, emulsifier, acid and modifier;

[0063] The asphalt selected in the S1 stage accounts for 30%-60% of the total mass of the emulsified asphalt, and the asphalt temperature is heated to 120℃-140℃.

[0064] S2: Raw material pretreatment stage:

[0065] The asphalt selected in the S1 stage is subjected to demulsification treatment;

[0066] There are two methods for demulsifying asphalt in the S2 stage: Method 1: slowly heat the asphalt over a low fire to prevent it from aging and deteriorating due to high temperature. In the absence of a thermometer, the temperature can be judged to be appropriate by observing whether the liquid surface is shiny, no longer bubbling, and whether there is blue smoke coming out, so as to obtain the asphalt after liquid demulsification. Method 2: liquid asphalt can also be stirred with solvents such as diesel and kerosene, or emulsified with water using an emulsifier to obtain emulsified asphalt. The different demulsification methods of asphalt in S2 are suitable for different processing environments during asphalt preparation, reduce the limitations during asphalt preparation, and facilitate the preparation of an appropriate proportion of emulsifier aqueous solution according to the quality of the emulsified asphalt.

[0067] S3: Soap preparation stage:

[0068] According to the emulsified asphalt obtained in the S2 stage, a suitable emulsifier and additives are selected to prepare an emulsifier aqueous solution;

[0069] The temperature of the emulsifier aqueous solution obtained in the S3 stage is maintained at 55℃-75℃ before entering the equipment. The independent temperature control design of S2 and S3 facilitates targeted heating according to the type of raw materials for asphalt heating, avoids temperature runaway during heating, ensures accurate temperature control, and avoids affecting the quality of asphalt preparation.

[0070] S4: Temperature control stage:

[0071] The temperatures during the preparation of S1, S2 and S3 are controlled separately;

[0072] Temperature control in S4 uses water heating and thermal oil heating;

[0073] The temperature of the inert gas introduced during the heating of the heat transfer oil is 310℃-350℃. When the temperature of S2 and S3 is used for heating and transportation, the inert gas is used as a protective layer or driving force to form a protective layer on the inner wall of the heating device of S2 and S3 to avoid coking of the outer asphalt and the heating device. At the same time, it can also increase the flow rate of asphalt with a certain viscosity to avoid local condensation when laying medium and high voltage power cables, affecting the overall solidification effect during laying.

[0074] S5: Fixed ratio stage:

[0075] The test personnel sampled and determined the ratio of the demulsified asphalt obtained by S2 and the emulsifier aqueous solution obtained by S2 to obtain the appropriate production ratio. Through the design of S5, it is convenient to accurately control the optimal ratio between the emulsified asphalt and the emulsifier aqueous solution, which is conducive to conducting tests in advance to obtain the finished product and avoid poor quality in subsequent large-scale asphalt preparation and mixing;

[0076] The particle size of S6 obtained by the crushing equipment is 0.1 to 5 microns, and the crushing equipment used in S6 is an emulsifier, so that the crushed particles can be more fully dispersed in the emulsifier aqueous solution.

[0077] S6: Emulsification of asphalt:

[0078] After the S5 ratio is reached, the asphalt and the emulsifier aqueous solution are put into the crushing equipment together. After the mechanical effects of the crushing equipment such as pressurization, shearing, and grinding, the asphalt is formed into uniform and fine particles, which are stably and evenly dispersed in the soap solution to form an oil-in-water asphalt emulsion.

[0079] S7: Storage of emulsified bitumen:

[0080] Emulsified asphalt passes through the cooling device and enters the storage tank.

[0081] Embodiment 3

[0082] S1: Raw material preparation stage:

[0083] Select asphalt, water, emulsifier, acid and modifier;

[0084] The asphalt selected in the S1 stage accounts for 30%-60% of the total mass of the emulsified asphalt, and the asphalt temperature is heated to 120℃-140℃.

[0085] S2: Raw material pretreatment stage:

[0086] The asphalt selected in the S1 stage is subjected to demulsification treatment;

[0087] There are two methods for demulsifying asphalt in the S2 stage: Method 1: slowly heat the asphalt over a low fire to prevent it from aging and deteriorating due to high temperature. In the absence of a thermometer, the temperature can be judged to be appropriate by observing whether the liquid surface is shiny, no longer bubbling, and whether there is blue smoke coming out, so as to obtain the asphalt after liquid demulsification. Method 2: liquid asphalt can also be stirred with solvents such as diesel and kerosene, or emulsified with water using an emulsifier to obtain emulsified asphalt. The different demulsification methods of asphalt in S2 are suitable for different processing environments during asphalt preparation, reduce the limitations during asphalt preparation, and facilitate the preparation of an appropriate proportion of emulsifier aqueous solution according to the quality of the emulsified asphalt.

[0088] S3: Soap preparation stage:

[0089] According to the emulsified asphalt obtained in the S2 stage, a suitable emulsifier and additives are selected to prepare an emulsifier aqueous solution;

[0090] The temperature of the emulsifier aqueous solution obtained in the S3 stage is maintained at 55℃-75℃ before entering the equipment. The independent temperature control design of S2 and S3 facilitates targeted heating according to the type of raw materials for asphalt heating, avoids temperature runaway during heating, ensures accurate temperature control, and avoids affecting the quality of asphalt preparation.

[0091] S4: Temperature control stage:

[0092] The temperatures during the preparation of S1, S2 and S3 are controlled separately;

[0093] Temperature control in S4 uses water heating and thermal oil heating;

[0094] The temperature of the inert gas introduced during the heating of the heat transfer oil is 310℃-350℃. When the temperature of S2 and S3 is used for heating and transportation, the inert gas is used as a protective layer or driving force to form a protective layer on the inner wall of the heating device of S2 and S3 to avoid coking of the outer asphalt and the heating device. At the same time, it can also increase the flow rate of asphalt with a certain viscosity to avoid local condensation when laying medium and high voltage power cables, affecting the overall solidification effect during laying.

[0095] S5: Fixed ratio stage:

[0096] The test personnel sampled and determined the ratio of the demulsified asphalt obtained by S2 and the emulsifier aqueous solution obtained by S2 to obtain the appropriate production ratio. Through the design of S5, it is convenient to accurately control the optimal ratio between the emulsified asphalt and the emulsifier aqueous solution, which is conducive to conducting tests in advance to obtain the finished product and avoid poor quality in subsequent large-scale asphalt preparation and mixing;

[0097] The particle size of S6 obtained by the crushing equipment is 0.1 to 5 microns, and the crushing equipment used in S6 is an emulsifier, so that the crushed particles can be more fully dispersed in the emulsifier aqueous solution.

[0098] S6: Emulsification of asphalt:

[0099] After the S5 ratio is reached, the asphalt and the emulsifier aqueous solution are put into the crushing equipment together. After the mechanical effects of the crushing equipment such as pressurization, shearing, and grinding, the asphalt is formed into uniform and fine particles, which are stably and evenly dispersed in the soap solution to form an oil-in-water asphalt emulsion.

[0100] S7: Storage of emulsified bitumen:

[0101] Emulsified asphalt passes through the cooling device and enters the storage tank.

[0102] S8: Asphalt paving use:

[0103] The asphalt stored in S8 is paved with inert gas as the medium during transportation and use;

[0104] The temperature of the inert gas in S8 is 300℃-400℃. Both water heating and heat transfer oil heating use inert gas as the medium to heat the asphalt. The ratio of inert gas to asphalt in S8 is 30:70. The temperature of the inert gas introduced in water heating is 300℃-400℃.

[0105] The asphalt obtained in Example 1 of Chinese patent CN202010795823.3 was used as a comparison and tested with the same standard. The results are as follows: the asphalt prepared according to the formula is Example 1 and Example 2, and Example 3 is the same as the content of the ingredients but different from the preparation method of this invention. The elongation value comparison result is shown in Figure 2 (the elongation length of asphalt at different temperatures), and the softening degree comparison result at different temperatures is shown in Figure 2. Figure 3 As shown in Figure 2, the flow velocity in the same time is as follows: Figure 4 As shown, in summary, the compactness of the asphalt prepared according to the present method is better than that of the comparative example and the asphalt prepared by different preparation methods.

[0106] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A process for preparing asphalt for medium and high voltage power cables, characterized in that: include: S1: Raw material preparation stage: Select asphalt, water, emulsifier, acid and modifier; S2: Raw material pretreatment stage: The asphalt selected in the S1 stage is subjected to demulsification treatment; S3: Soap preparation stage: According to the emulsified asphalt obtained in the S2 stage, a suitable emulsifier and additives are selected to prepare an emulsifier aqueous solution; S4: Temperature control stage: The temperatures during the preparation of S1, S2 and S3 are controlled separately; S5: Fixed ratio stage: The test personnel sampled and determined the ratio of the demulsified asphalt obtained from S2 and the emulsifier aqueous solution obtained from S2 to obtain the appropriate production ratio; S6: Emulsification of asphalt: After the S5 ratio is reached, the asphalt and the emulsifier aqueous solution are put into the crushing equipment together. After the mechanical action of the crushing equipment such as pressurization, shearing, grinding, etc., the asphalt is formed into uniform and fine particles, which are stably and evenly dispersed in the soap solution to form an oil-in-water asphalt emulsion. S7: Storage of emulsified bitumen: Emulsified asphalt passes through the cooling device and enters the storage tank; S8: Asphalt paving use: The asphalt stored in S8 is paved using inert gas as the medium during transportation.

2. The asphalt preparation process for medium and high voltage power cables according to claim 1, characterized in that: The asphalt selected in the S1 stage accounts for 30%-60% of the total mass of the emulsified asphalt, and the asphalt temperature is relatively high at 120°C-140°C.

3. The asphalt preparation process for medium and high voltage power cables according to claim 1, characterized in that: There are two methods for demulsifying asphalt in the S2 stage: Method 1: slowly heat the asphalt over a low fire to prevent it from aging and deteriorating due to high temperature. In the absence of a thermometer, the temperature can be judged to be appropriate by observing whether the liquid surface is shiny, no longer bubbling, and whether blue smoke is emitted, thereby obtaining the asphalt after liquid demulsification; Method 2: the liquid asphalt can also be stirred with solvents such as diesel and kerosene, or emulsified with water using an emulsifier to obtain emulsified asphalt.

4. The asphalt preparation process for medium and high voltage power cables according to claim 1, characterized in that: The temperature of the emulsifier aqueous solution obtained in the S3 stage is maintained at 55° C.-75° C. before entering the equipment.

5. The asphalt preparation process for medium and high voltage power cables according to claim 1, characterized in that: The temperature control in S4 adopts water heating and heat transfer oil heating, and both water heating and heat transfer oil heating use inert gas as the medium to heat the asphalt.

6. The asphalt preparation process for medium and high voltage power cables according to claim 1, characterized in that: The particle size of the particles obtained by the crushing equipment in S5 is 0.1 to 5 microns, and the crushing equipment used in S5 is an emulsifier.

7. The asphalt preparation process for medium and high voltage power cables according to claim 1, characterized in that: The cooling device used for the emulsified asphalt in S7 is circulating water cooling and dry ice cooling, and the storage pipe used in S7 is equipped with a built-in stirring device, and the stirring device adopts timed stirring.

8. The asphalt preparation process for medium and high voltage power cables according to claim 5, characterized in that: The temperature of the inert gas in S8 is 300°C-400°C.

9. The asphalt preparation process for medium and high voltage power cables according to claim 8, characterized in that: The ratio of the S8 inert gas to asphalt is 30:70, and the temperature of the inert gas introduced during the water heating is 300°C-400°C.

10. The asphalt preparation process for medium and high voltage power cables according to claim 8, characterized in that: The temperature of the inert gas introduced during the heating of the thermal oil is 310°C-350°C.