An acid-resistant organic coating for reactive metal surfaces and its preparation method
By forming a nanosphere coating of dynamic borate ester bonds and perfluoroalkyl propylene oxide on the surface of reactive metals, the problem of instability of existing coatings in acidic environments is solved, the properties of the metal are maintained and the acid corrosion resistance is improved, making it suitable for the protection of reactive metals.
Patent Information
- Application Number
- CN202411195697.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-08-29
AI Technical Summary
Existing organic coatings on reactive metal surfaces, while ensuring acid resistance, affect the properties of the reactive metals themselves and are not stable enough in acidic environments.
A hydrophobic coating of dynamic borate ester bonds and perfluoroalkyl propylene oxide is used to form a uniformly distributed nanosphere structure on the surface of an active metal through an epoxy addition reaction. The coating layer is formed by utilizing the electron affinity and long-range force between fluorine atoms and the metal surface.
It maintains the stability of active metals in acidic environments, reduces the impact on metal properties, improves the acid corrosion resistance of the coating and its compatibility with nitrogen-containing compounds, and is suitable for the storage and application of active metals.
Smart Images

Figure CN118931242B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an acid-resistant organic coating for reactive metal surfaces and its preparation method, belonging to the field of high-performance polymer technology. Background Technology
[0002] Reactive metals, also known as active metals, are metals that precede hydrogen in the activity series of metals. They possess high chemical reactivity and readily react with other substances. Reactive metals mainly exist in nature as compounds because they readily react with oxygen, water vapor, hydrogen sulfide, and other substances to form compounds. Reactive metals include lithium (Li), calcium (Ca), magnesium (Mg), and aluminum (Al). Due to their high reactivity, reactive metals have important applications in many fields; however, their excessive chemical reactivity significantly increases the difficulty of storage. This invention uses the application of energetic fuels as an example. For instance, aluminum-lithium alloys have strong application potential in the propellant field due to their high heat of combustion and low ignition point. However, because lithium is highly reactive, it easily undergoes chemical reactions, leading to deterioration and even hazards. Therefore, appropriate safety measures are needed to handle and use these materials.
[0003] Organic coatings on reactive metal surfaces are a common protective method. This method involves applying an organic material coating to the metal surface, which provides protection against corrosion in various environments. Acid resistance is a key characteristic of organic coatings for reactive metals, meaning that the coating can maintain its structure and function in acidic environments, thus protecting the metal substrate from corrosion.
[0004] Currently available acid-resistant organic coatings include organic compounds such as fluorosilanes and siloxanes. Almost all existing acid-resistant organic coatings consist of a thick and very dense protective layer. This structure reduces the compatibility of active metals with other organic groups (such as azide groups) and also affects the properties of the active metal itself, such as its heat of combustion. Therefore, the problem of how to ensure the acid resistance of active metal organic coatings while minimizing the impact on the properties of the active metal itself urgently needs to be solved.
[0005] To address this, researchers attempted to achieve this goal by altering the structure of the coating. For example, coating reactive metal surfaces with phytic acid resulted in the formation of uniformly distributed nanospheres, effectively reducing the coating thickness and the amount of organic matter required. However, metals coated with phytic acid could not remain stable in acidic environments. Summary of the Invention
[0006] In view of this, the purpose of this invention is to provide an acid-resistant organic coating for active metal surfaces and its preparation method. The coating ensures the stability of the active metal under acidic conditions while possessing a nanosphere structure. Regarding acid resistance, the coating itself is based on dynamic borate ester bonds and the hydrophobicity of perfluoroalkyl propylene oxide, which are organically combined through an epoxy addition reaction, resulting in an organic coating that is both water-resistant and acid-resistant. In terms of microstructure, the coating forms a uniformly distributed granular microsphere structure on the active metal surface. This structure allows for a thinner coating layer with minimal impact on the metal's properties, while boron atoms are distributed on the outer layer of the microspheres. Perfluoroalkyl propylene oxide contains a large amount of fluorine. On the one hand, the significant difference in electronegativity between fluorine and active metals allows fluorine atoms to have a strong electron affinity for the active metal surface. On the other hand, the long-range forces between the fluoride and the metal surface cause the perfluorinated compound molecules to be tightly adsorbed onto the metal surface. Through epoxy addition reaction, acid-resistant dynamic borate ester bonds can be firmly adsorbed onto the outermost layer, thus forming a strong and effective coating layer. The resulting organic acid-resistant coating is of great significance for protecting metals from acid corrosion and improving the safety and economy of industrial applications.
[0007] To achieve the above objectives, the technical solution of the present invention is as follows.
[0008] An acid-resistant organic coating for reactive metal surfaces, wherein the coating material has the following structural formula:
[0009] n is an integer from 5 to 8;
[0010] The coating material is uniformly distributed on the surface of the active metal in a granular structure.
[0011] Preferably, per 100nm 2 The active metal surface is coated with 12 to 15 spherical particles with a diameter of 20 to 25 nm.
[0012] Preferably, the coating material is adsorbed onto the surface of the active metal through the electron affinity and long-range force between fluorine atoms and the active metal.
[0013] Preferably, the active metal powder is an elemental powder or alloy powder of lithium, calcium, magnesium and aluminum.
[0014] Preferably, the active metal is aluminum-lithium alloy powder, and the mass fraction of lithium is 5% to 7%.
[0015] A method for preparing an acid-resistant organic coating for an active metal surface according to the present invention, comprising the following steps:
[0016] (1) Prepare a dehydration product of monohydroxy substituted phenylboronic acid, dissolve the dehydration product in ethyl acetate to obtain a monohydroxy substituted phenylboronic acid dehydration product solution; dissolve perfluoroalkyl propylene oxide in ethyl acetate to obtain a perfluoroalkyl propylene oxide solution;
[0017] (2) Disperse the active metal powder in the first organic solvent to obtain an active metal powder dispersion; add a perfluoroalkyl propylene oxide solution, add a catalyst at 40-60°C with stirring, and then add a monohydroxy-substituted phenylboronic acid dehydration product solution at a rate of one drop every 2-3 seconds, and continue stirring for 4-5 hours. After the reaction is completed, separate and dry to obtain an acid-resistant active metal surface organic coating.
[0018] Preferably, in step (1), the monohydroxy substituted phenylboronic acid is 4-hydroxyphenylboronic acid or 3-hydroxyphenylboronic acid; the perfluoroalkyl propylene oxide is 3-(perfluorohexyl)propylene oxide, 3-(perfluoropentyl)propylene oxide, 3-(perfluoroheptyl)propylene oxide or 3-(perfluorooctyl)propylene oxide.
[0019] Preferably, in step (1), when preparing the dehydrated product of monohydroxy-substituted phenylboronic acid, the monohydroxy-substituted phenylboronic acid is dissolved in a second organic solvent, refluxed at 50–60°C for 12–15 h, and then distilled under reduced pressure at 40–45°C to obtain the dehydrated product of monohydroxy-substituted phenylboronic acid. More preferably, the second organic solvent is one or more of tetrahydrofuran, ethyl acetate, and isopropanol. The ratio of monohydroxy-substituted phenylboronic acid to the second organic solvent is 2 g: 54–58 mL.
[0020] Preferably, in step (1), the ratio of the amount of the monohydroxy-substituted phenylboronic acid dehydration product to ethyl acetate in the monohydroxy-substituted phenylboronic acid dehydration product solution is 0.4 g: 20-30 mL; and the ratio of the amount of the perfluoroalkyl propylene oxide solution to ethyl acetate is 1.32-1.40 g: 20-30 mL.
[0021] Preferably, in step (2), the mass ratio of the active metal powder to the dehydration product of monohydroxy substituted phenylboronic acid is 1:0.2 to 0.3; and the molar ratio of perfluoroalkyl propylene oxide to the dehydration product of monohydroxy substituted phenylboronic acid is 3 to 6:1.
[0022] Preferably, in step (2), the first organic solvent is one or more of tetrahydrofuran, ethyl acetate, and N,N-dimethylformamide.
[0023] Preferably, in step (2), the catalyst is a boron trifluoride diethyl ether solution with a mass fraction of 45% to 50%.
[0024] Preferably, in step (2), the drying temperature is 60-80℃ and the time is 8-12h.
[0025] Beneficial effects
[0026] This invention provides an acid-resistant organic coating for reactive metal surfaces. The coating material ensures the stability of the reactive metal under acidic conditions through the pH stability of dynamic borate bonds. Its multi-microsphere encapsulation structure largely preserves the properties of the reactive metal and improves compatibility with nitrogen-containing compounds. Furthermore, the strong hydrophobicity of perfluoroalkyl propylene oxide further enhances the stability of the organic coating in humid acidic environments. This material exhibits excellent stability, effectively maintaining its stability at both low and normal temperatures, and remains stable whether placed in air or water. It can be applied to acid-resistant reactive metals. Reactive metals coated with this organic coating demonstrate excellent acid resistance, remaining stable in strong acid solutions with a pH less than 2 for up to one day, and can be stored long-term under acidic conditions with a pH greater than 2.
[0027] This invention provides an acid-resistant organic coating for reactive metal surfaces, wherein the coating surface has a granular structure, with each 100 nm layer having a specific particle size distribution. 2 The coating contains 12–15 near-spherical particles with a diameter of 20–25 nm, ensuring that it provides acid resistance while minimizing the impact on the properties of the active metal itself. The particle surface is rich in boron. Between the coating and the metal, the significant difference in electronegativity between fluorine and the active metal allows fluorine atoms to have a strong electron affinity for the metal surface. Furthermore, the long-range forces between the fluoride and the metal surface ensure that the fluorine compound molecules are tightly adsorbed onto the metal surface.
[0028] This invention provides a method for preparing an acid-resistant organic coating on an active metal surface. The coating material is obtained by the dehydration of a monohydroxy-substituted phenylboronic acid product and the epoxy addition of a perfluorinated substituted alkyl propylene oxide. The monohydroxy-substituted phenylboronic acid is first dehydrated and condensed into a trimer. The boron-oxygen bonds and the outer phenolic hydroxyl groups in the trimer can withstand acid corrosion and protect the metal itself from acid corrosion. The perfluorinated substituted alkyl propylene oxide containing a large amount of fluorine is a hydrophobic material and can effectively prevent the reaction between water molecules and the metal.
[0029] This invention provides a method for preparing an acid-resistant organic coating for active metal surfaces. The -OH group on the boric acid in monohydroxy-substituted phenylboronic acid undergoes dehydration condensation in a heated organic solvent. After the reaction, the solvent is evaporated to become a dehydrated product, which then undergoes an epoxy ring-opening addition reaction with a perfluorinated alkyl propylene oxide under catalytic conditions to form a coating on the metal surface. The finished product is then obtained by vacuum filtration and drying. The method is simple, the experimental formula can be modified according to production needs, and it can be industrialized.
[0030] This invention provides a method for preparing an acid-resistant organic coating on an active metal surface. In this method, the dropping rate of the dehydration product of monohydroxy-substituted phenylboronic acid must be strictly controlled. If the rate is too fast, it will cause local accumulation of raw materials and uneven distribution, which will affect the distribution of the final coating material. Attached Figure Description
[0031] Figure 1 The image shows the SEM results of the aluminum-lithium alloy powder with an organic coating in Example 1.
[0032] Figure 2 This is a diagram showing the result of placing the aluminum-lithium alloy powder with an organic coating in hydrochloric acid solution in Example 1.
[0033] Figure 3 The image shows the results of placing the aluminum-lithium alloy powder with an organic coating in an acidic solution for 7 days in Example 1.
[0034] Figure 4 The image shows the water contact angle of the aluminum-lithium alloy powder in Example 1.
[0035] Figure 5 This is a diagram showing the water contact angle of the aluminum-lithium alloy powder with an organic coating in Example 1. Detailed Implementation
[0036] The present invention will be further described in detail below with reference to specific embodiments.
[0037] Example 1
[0038] (1) Prepare a 5 wt% tetrahydrofuran solution of 4-hydroxyphenylboronic acid, heat to 50 °C, stir, and add a reflux device. React for 12 h, then remove the tetrahydrofuran by vacuum distillation at 40 °C to obtain the dehydrated product of 4-hydroxyphenylboronic acid. Dissolve 1.32 g of 3-(perfluorohexyl)propoxide in 20 mL of ethyl acetate solution to obtain a 3-(perfluorohexyl)propoxide solution.
[0039] (2) Take 2g of aluminum-lithium alloy powder (lithium mass fraction of 5%) and place it in ethyl acetate, then put it into the reaction apparatus, add 3-(perfluorohexyl)propane oxide solution, heat to 60℃ and stir at a stirring speed of about 500r / min, and add 600μl of 48% boron trifluoride diethyl ether solution to the solution.
[0040] (3) Dissolve 0.4 g of the dehydration product of 4-hydroxyphenylboronic acid in 20 mL of ethyl acetate solution. Using a separatory funnel, add the product to the reaction apparatus at a rate of one drop every 2 seconds, so that the dehydration product can undergo a dehydration condensation reaction with 3-(perfluorohexyl)propane oxide. The reaction lasts for 4 hours. After the reaction is completed, vacuum filter the product and then dry it in a vacuum oven for 8 hours at a temperature of 65°C to obtain acid-resistant aluminum-lithium alloy powder with an organic coating.
[0041] Infrared and nuclear magnetic resonance tests showed that the structural formula of the organic coating material is:
[0042]
[0043] like Figure 1 As shown, the aluminum-lithium alloy powder has granular material adhering to its surface, with a density of 100 nm per 100 nm. 2 It contains 12 to 15 spherical particles with a diameter of 20 to 25 nm.
[0044] like Figure 2 As shown, when the aluminum-lithium alloy powder with the attached organic coating is placed in a hydrochloric acid solution with a pH of 1 to 2, the aluminum-lithium alloy powder with the attached organic coating can remain stable in a strong acid solution with a pH of less than 2 for 1 hour.
[0045] The results of placing the aluminum-lithium alloy powder with the attached organic coating in an acetic acid solution with a pH of 3-4 for 7 days are as follows: Figure 3 As shown, the aluminum-lithium alloy powder with an attached organic coating can be stored for a long time under acidic conditions with a pH greater than 2.
[0046] like Figure 4 The water contact angles of the aluminum-lithium alloy powder shown are 27.6° on the left and 26.9° on the right. Figure 5 The water contact angles of the aluminum-lithium alloy powder with the attached organic coating are shown to be 62.4° on the left and 63.9° on the right.
[0047] The calorific value of aluminum-lithium alloy powder is 31.401 kJ / g, while the calorific value of aluminum-lithium alloy powder with an attached organic coating is 31.063 kJ / g.
[0048] Example 2
[0049] (1) Prepare a 5 wt% isopropanol solution of 3-hydroxyphenylboronic acid, heat to 50 °C, stir, and add a reflux device. React for 12 h, then remove isopropanol by vacuum distillation at 40 °C to obtain the dehydrated product of 3-hydroxyphenylboronic acid. Dissolve 1.40 g of 3-(perfluorohexyl)propoxide in 30 mL of ethyl acetate solution to obtain a 3-(perfluorohexyl)propoxide solution.
[0050] (2) Take 2g of aluminum-lithium alloy powder (lithium mass fraction of 5%) and place it in ethyl acetate, then put it into the reaction apparatus, add 3-(perfluorohexyl) propylene oxide solution, heat to 50℃ and stir, stirring speed is about 500r / min, add 600μl of 48% boron trifluoride diethyl ether solution to the solution.
[0051] (3) Dissolve 0.4 g of the dehydration product of 3-hydroxyphenylboronic acid in 30 mL of ethyl acetate solution. Using a separatory funnel, add the product to the reaction apparatus at a rate of one drop every 2 seconds, so that the dehydration product reacts with 3-(perfluorohexyl)propane oxide in a dehydration condensation reaction. The reaction lasts for 4 hours. After the reaction is completed, vacuum filter the product and then dry it in a vacuum oven at 65 °C for 8 hours to obtain acid-resistant aluminum-lithium alloy powder with an organic coating.
[0052] Infrared and nuclear magnetic resonance tests showed that the structural formula of the organic coating material is:
[0053]
[0054] The aluminum-lithium alloy powder has granular material adhering to its surface, with each 100nm... 2 It contains 12 to 15 spherical particles with a diameter of 20 to 25 nm.
[0055] When the aluminum-lithium alloy powder with the attached organic coating is placed in a hydrochloric acid solution with a pH of 1 to 2, the aluminum-lithium alloy powder with the attached organic coating can remain stable in a strong acid solution with a pH of less than 2 for 1 hour.
[0056] The results of placing the aluminum-lithium alloy powder with the attached organic coating in an acetic acid solution with a pH of 3-4 for 7 days showed that the aluminum-lithium alloy powder with the attached organic coating could be stored for a long time under acidic conditions with a pH greater than 2.
[0057] In summary, the invention includes, but is not limited to, the above embodiments. Any equivalent substitutions or partial improvements made under the spirit and principles of this invention shall be considered to be within the protection scope of this invention.
Claims
1. An acid-resistant organic coating for active metal surfaces, characterized in that: The coating is formed from a coating material with the following structural formula: or n is an integer from 5 to 8; The coating material is uniformly distributed on the surface of the active metal in a granular structure.
2. The acid-resistant organic coating for active metal surfaces as described in claim 1, characterized in that: per 100nm 2 The active metal surface is coated with 12-15 spherical particles with a diameter of 20-25 nm.
3. A method for preparing an acid-resistant organic coating for an active metal surface as described in claim 1 or 2, characterized in that: The method steps include: (1) Prepare the dehydration product of monohydroxy substituted phenylboronic acid, dissolve the dehydration product in ethyl acetate to obtain a monohydroxy substituted phenylboronic acid dehydration product solution; dissolve perfluoroalkyl propylene oxide in ethyl acetate to obtain a perfluoroalkyl propylene oxide solution; (2) Disperse the active metal powder in the first organic solvent to obtain an active metal powder dispersion; add a perfluoroalkyl propylene oxide solution, add a catalyst at 40~60℃ with stirring, and then add a monohydroxy substituted phenylboronic acid dehydration product solution at a rate of one drop every 2~3 seconds. Continue stirring for 4~5 hours. After the reaction is completed, separate and dry to obtain an acid-resistant active metal surface organic coating.
4. The method for preparing an acid-resistant organic coating for an active metal surface as described in claim 3, characterized in that: In step (1), the monohydroxy-substituted phenylboronic acid is 4-hydroxyphenylboronic acid or 3-hydroxyphenylboronic acid; the perfluoroalkyl propylene oxide is 3-(perfluorohexyl)propylene oxide, 3-(perfluoropentyl)propylene oxide, 3-(perfluoroheptyl)propylene oxide or 3-(perfluorooctyl)propylene oxide; in the monohydroxy-substituted phenylboronic acid dehydration product solution, the ratio of the monohydroxy-substituted phenylboronic acid dehydration product to ethyl acetate is 0.4 g: 20~30 mL; in the perfluoroalkyl propylene oxide solution, the ratio of the perfluoroalkyl propylene oxide to ethyl acetate is 1.32~1.40 g: 20~30 mL.
5. The method for preparing an acid-resistant organic coating for an active metal surface as described in claim 3, characterized in that: In step (1), when preparing the dehydrated product of monohydroxy-substituted phenylboronic acid, the monohydroxy-substituted phenylboronic acid is dissolved in a second organic solvent, refluxed at 50~60℃ for 12~15h, and distilled under reduced pressure at 40~45℃ to obtain the dehydrated product of monohydroxy-substituted phenylboronic acid.
6. The method for preparing an acid-resistant organic coating for an active metal surface as described in claim 5, characterized in that: The second organic solvent is one or more of tetrahydrofuran, ethyl acetate, and isopropanol; the ratio of monohydroxy substituted phenylboronic acid to the second organic solvent is 2g:54~58mL.
7. The method for preparing an acid-resistant organic coating for an active metal surface as described in claim 3, characterized in that: In step (2), the mass ratio of the active metal powder to the dehydration product of monohydroxy substituted phenylboronic acid is 1:0.2~0.3; the molar ratio of perfluoroalkyl propylene oxide to the dehydration product of monohydroxy substituted phenylboronic acid is 3~6:
1.
8. The method for preparing an acid-resistant organic coating for an active metal surface as described in claim 3, characterized in that: In step (2), the first organic solvent is one or more of tetrahydrofuran, ethyl acetate, and N,N-dimethylformamide; The catalyst is a boron trifluoride diethyl ether solution with a mass fraction of 45%~50%; The drying temperature is 60~80℃, and the time is 8~12h.
Citation Information
Patent Citations
Composite material of resin-fluorine-containing boric acid composite particles
CN106459593A
Layer-by-layer self-assembled energetic aluminum powder as well as preparation method and application thereof