Black cloth scraping adhesive cement for base cloth in anti-static rubber shoe sponge as well as preparation and application methods of black cloth scraping adhesive cement
By preparing a black scraping adhesive paste for the sponge insole of antistatic rubber shoes, the problem of adhesive penetration between the insole fabric and the sponge rubber was solved, achieving antistatic function and high bonding strength, and improving the appearance and service life of the rubber shoes.
Patent Information
- Application Number
- CN202411236485.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
AI Technical Summary
The bonding process between the insole fabric and sponge rubber in existing rubber shoes is prone to glue seepage quality problems, and traditional adhesives do not have charge conduction function, leading to static electricity accumulation, which affects the appearance and service life.
The black coating adhesive used in the antistatic rubber shoe sponge insole is composed of natural latex, kaolin, sodium silicate, potassium hydroxide, sodium carboxymethyl cellulose, leveling agent, and penetrant. It is prepared through a specific process and coated onto the rubber shoe insole to ensure bonding strength and charge conduction capability.
This technology achieves effective bonding between the insole fabric and sponge rubber of rubber shoes, provides anti-static properties, improves production quality and service life, and reduces production costs.
Smart Images

Figure BDA0005027870340000051 
Figure BDA0005027870340000052 
Figure BDA0005027870340000061
Abstract
Description
Technical Field
[0001] The invention relates to an antistatic rubber shoe sponge midsole cloth black scraper slurry and a preparation and application method thereof, belonging to the technical field of rubber processing. Background Art
[0002] In order to obtain aesthetic effects and increase the wearing life of rubber shoes, the side of the inner sole surface of the rubber shoes that contacts the human body is usually isolated by cloth and sponge rubber. In order to achieve the bonding of cloth and sponge rubber, it is required to ensure that there is no quality problem of glue penetration on the cloth surface. For this reason, a layer of rubber glue with high filling performance must be applied on the cloth on the bonding surface with the sponge rubber so that the gaps in the cloth fibers are completely filled with glue to ensure that there is no quality accident of glue penetration during the manufacturing process of rubber shoes. This rubber glue is usually made of natural rubber compound swollen with gasoline, and its resistance value is very large, and it does not have the function of charge conduction. However, the water-based glue usually made of latex has low consistency. Although it has the ability of charge conduction, it cannot be used as the scraping glue for the midsole cloth because it will cause glue penetration when applied on the rubber shoe bottom cloth and the bottom cloth will cause serious adhesion and deformation during the punching process.
[0003] Latex slurry needs to use kaolin as a filler to ensure the ability of charge permeation, but adding kaolin to latex can easily cause latex demulsification and agglomeration, resulting in slurry damage and loss of application function. The combination of sodium silicate and natural latex slurry can improve the stiffness of the slurry under moisture-free conditions, improve the stiffness of the midsole fabric for shoes attached to the slurry, and facilitate process operations.
[0004] Therefore, the invention of water-based antistatic scraper cloth glue has urgent practical significance in the process of producing antistatic rubber shoes. Summary of the invention
[0005] The purpose of the present invention is to provide an anti-static rubber shoe sponge midsole cloth black scraper glue and its preparation and application method. The black scraper glue has anti-static function, good bonding strength, is non-toxic and environmentally friendly, can improve production quality, and overcome the shortcomings of the prior art.
[0006] The technical scheme of the present invention is as follows: the black scraping cloth slurry for the midsole cloth of the antistatic rubber shoe sponge is prepared from the following raw materials in parts by weight: 100 parts of natural latex, 15-25 parts of kaolin, 43-45 parts of soft water, 10-14 parts of sodium silicate, 1.0-2.0 parts of mildewproof agent BCM, 0.05-0.15 parts of potassium hydroxide, 2.5-3.5 parts of sodium carboxymethyl cellulose, 0.3-0.5 parts of peregrin, 0.5-1.5 parts of penetrant and 0.4-0.6 parts of black slurry.
[0007] The aforementioned anti-static rubber shoe sponge midsole cloth black scraper slurry is made of the following raw materials in parts by weight: 100 parts of natural latex, 20 parts of kaolin, 44 parts of soft water, 12 parts of sodium silicate, 1.5 parts of mildew preventer BCM, 0.1 parts of potassium hydroxide, 3 parts of sodium carboxymethyl cellulose, 0.4 parts of perglase, 1.0 parts of penetrant, and 0.5 parts of black slurry.
[0008] In the aforementioned anti-static rubber shoe sponge midsole cloth black scraper glue, the specifications of sodium silicate are: a sodium silicate aqueous solution with a silicon dioxide content ≥24.6% and a Baume degree of 0.35-0.37; the solid content of natural latex is 60%; the specification of sodium carboxymethyl cellulose is FH9; the specification of potassium oxide is industrial grade; the specification of Pingpingjia is type O; the model of the penetrant is JFC; and the model of the black paste is 8501 paint black paste.
[0009] The preparation method of the black scraper mortar for the sponge midsole of antistatic rubber shoes comprises taking each component according to the above-mentioned weight parts;
[0010] S1: preparing cellulose mother liquor: putting 34 / 44 parts of soft water, all the sodium carboxymethyl cellulose, mildew inhibitor BCM, Periga and penetrant into a blender, stirring slowly and adding all the potassium hydroxide, stirring until the sodium carboxymethyl cellulose is evenly dispersed and has no agglomeration to form a thick liquid, thereby obtaining a cellulose mother liquor;
[0011] S2 scraper glue manufacturing:
[0012] S2-1 Preparation of impregnated clay: Add all the kaolin, 5 / 44 parts of soft water, and all the sodium carbonate into a mixing barrel and stir until the kaolin is evenly moistened to obtain 37 parts of impregnated clay;
[0013] S2-2 Preparation of scraping cloth slurry: stir cellulose mother liquor and 10% natural latex in the slurry mixing barrel, stir well and evenly, then add 20% natural latex, stir well and evenly, then add the remaining natural latex, stir well and evenly to obtain a latex mixture; then add impregnated clay to the mixture, wash the impregnated clay residue twice with the remaining soft water on the mixing barrel wall impregnated with clay and add it to the latex mixture, add black slurry, stir until the material is fully uniform, and obtain the black scraping cloth slurry for anti-static rubber shoe sponge midsole cloth.
[0014] The application method of the black scraping cloth mortar for the anti-static rubber shoe sponge midsole cloth is as follows: within 48 hours after the black scraping cloth mortar for the anti-static rubber shoe sponge midsole cloth is prepared, the black scraping cloth mortar for the anti-static rubber shoe sponge midsole cloth is evenly scraped on the rubber shoe midsole cloth to form a mortar layer with a thickness of 0.2 to 0.4 mm, and the coating area is the cloth surface where the rubber shoe midsole cloth is bonded to the rubber.
[0015] In the aforementioned application method of the antistatic rubber shoe sponge midsole cloth black scraping cloth mortar, the antistatic rubber shoe sponge midsole cloth black scraping cloth mortar should be stored for more than 3 hours after preparation before use.
[0016] Beneficial effects of the invention: The invention adopts the above-mentioned technical scheme. Compared with the prior art, the anti-static rubber shoe sponge midsole cloth black scraper glue of the invention has anti-static function, good bonding strength, non-toxic and environmentally friendly, and the method of the method can improve production quality, and is simple and easy to operate, low cost, and good product use effect. DETAILED DESCRIPTION
[0017] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.
[0018] Embodiment 1 of the present invention: Antistatic rubber shoe sponge midsole cloth black scraper slurry is made of the following raw materials in parts by weight: 100 parts of natural latex, 20 parts of kaolin, 44 parts of soft water, 12 parts of sodium silicate, 1.5 parts of mildew preventer BCM, 0.1 parts of potassium hydroxide, 3 parts of sodium carboxymethyl cellulose, 0.4 parts of perglase, 1.0 parts of penetrant, and 0.5 parts of black slurry.
[0019] Embodiment 2 of the present invention: Antistatic rubber shoe sponge midsole cloth black scraper slurry is made of the following raw materials in parts by weight: 100 parts of natural latex, 22 parts of kaolin, 44 parts of soft water, 13 parts of sodium silicate, 1.8 parts of mildew preventer BCM, 0.12 parts of potassium hydroxide, 2.8 parts of sodium carboxymethyl cellulose, 0.4 parts of perglase, 1.0 parts of penetrant, and 0.5 parts of black slurry.
[0020] Embodiment 3 of the present invention: Antistatic rubber shoe sponge midsole cloth black scraper slurry is made of the following raw materials in parts by weight: 100 parts of natural latex, 15 parts of kaolin, 43 parts of soft water, 10 parts of sodium silicate, 1.0 part of mildew preventer BCM, 0.05 parts of potassium hydroxide, 2.5 parts of sodium carboxymethyl cellulose, 0.3 parts of perglase, 0.5 parts of penetrant, and 0.4 parts of black slurry.
[0021] Embodiment 4 of the present invention: Antistatic rubber shoe sponge midsole cloth black scraper slurry is made of the following raw materials in parts by weight: 100 parts of natural latex, 25 parts of kaolin, 45 parts of soft water, 14 parts of sodium silicate, 2.0 parts of mildew inhibitor BCM, 0.15 parts of potassium hydroxide, 3.5 parts of sodium carboxymethyl cellulose, 0.5 parts of perglase, 1.5 parts of penetrant, and 0.6 parts of black slurry.
[0022] In the above embodiment, the specifications of sodium silicate are: a sodium silicate aqueous solution with a silicon dioxide content of ≥24.6% and a Baume degree of 0.35-0.37; the solid content of natural latex is 60%; the specification of sodium carboxymethyl cellulose is FH9; the specification of potassium oxide is industrial grade; the specification of peregrin is type O; the model of the penetrant is JFC; and the model of the black paste is 8501 paint black paste.
[0023] The preparation method of the anti-static rubber shoe sponge midsole cloth black scraper cloth slurry of the above embodiment is to take each component according to the above weight parts;
[0024] S1: preparing cellulose mother liquor: putting 34 / 44 parts of soft water, all the sodium carboxymethyl cellulose, mildew inhibitor BCM, Periga and penetrant into a blender, stirring slowly and adding all the potassium hydroxide, stirring until the sodium carboxymethyl cellulose is evenly dispersed and has no agglomeration to form a thick liquid, thereby obtaining a cellulose mother liquor;
[0025] S2 scraper glue manufacturing:
[0026] S2-1 Preparation of impregnated clay: Add all the kaolin, 5 / 44 parts of soft water, and all the sodium carbonate into a mixing barrel and stir until the kaolin is evenly moistened to obtain 37 parts of impregnated clay;
[0027] S2-2 Preparation of scraping cloth slurry: stir cellulose mother liquor and 10% natural latex in the slurry mixing barrel, stir well and evenly, then add 20% natural latex, stir well and evenly, then add the remaining natural latex, stir well and evenly to obtain a latex mixture; then add impregnated clay to the mixture, wash the impregnated clay residue twice with the remaining soft water on the mixing barrel wall impregnated with clay and add it to the latex mixture, add black slurry, stir until the material is fully uniform, and obtain the black scraping cloth slurry for anti-static rubber shoe sponge midsole cloth.
[0028] The application method of the black scraping cloth slurry of the anti-static rubber shoe sponge bottom cloth in the above embodiment is that within 48 hours after the preparation of the black scraping cloth slurry of the anti-static rubber shoe sponge bottom cloth, the black scraping cloth slurry of the anti-static rubber shoe sponge bottom cloth is evenly scraped on the rubber shoe bottom cloth to form a slurry layer with a thickness of 0.2-0.4mm, and the brushing area is the cloth surface where the rubber shoe bottom cloth and the rubber are bonded, so as to prevent the unvulcanized rubber from penetrating through the bottom cloth fiber to form glue on the use surface of the bottom cloth during the rubber shoe manufacturing process, thereby improving the appearance quality of the rubber shoe and increasing the warmth-keeping function of the rubber shoe. The resistance of the cloth after scraping is between 0.01-0.1MΩ, which meets the resistance requirements of the anti-static shoe components.
[0029] After the preparation of the anti-static rubber shoe sponge midsole cloth and black scraper cloth slurry, it should be stored for more than 3 hours before being distributed and used, and allowed to flow into the next process for use.
[0030] In order to further verify the effect of the present invention, the following experiments were carried out:
[0031] 1. Research on the optimal ratio of raw materials
[0032] Table 1
[0033]
[0034] Table 1 continued
[0035]
[0036]
[0037] According to the test results in Table 1, the best formula is: 100 parts of natural latex, 20 parts of kaolin, 44 parts of soft water, 12 parts of sodium carbonate, 1.5 parts of mildew inhibitor BCM, 0.1 parts of potassium hydroxide, 3 parts of sodium carboxymethyl cellulose, 0.4 parts of perchlorate, 1.0 parts of penetrant, and 0.5 parts of black pulp.
[0038] 2. Pulping Technology Research
[0039] Table 2
[0040]
[0041]
[0042] By comparing several process flows in Table 2, it is concluded that the best manufacturing process is:
[0043] Step 1: Prepare cellulose mother liquor: put 34 parts of soft water, 3 parts of sodium carboxymethyl cellulose, 1.5 parts of mildew preventer BCM, 0.4 parts of peregrin, and 1.0 parts of penetrant into a blender, slowly stir and add 0.1 parts of potassium hydroxide, stir to obtain a thick liquid with sodium carboxymethyl cellulose evenly dispersed and without agglomeration, and obtain 40.0 parts of cellulose mother liquor;
[0044] Step 2: Scrape cloth glue production:
[0045] (1) Preparation of impregnated clay: Add 20 parts of kaolin, 5 parts of soft water, and 12 parts of sodium silicate into a mixing barrel and stir until the kaolin is evenly moistened to obtain 37 parts of impregnated clay.
[0046] (2) Preparation of scraping cloth slurry: Add 40 parts of cellulose mother liquor and 10 parts of natural latex into the slurry mixing barrel, stir well and evenly, then add 20 parts of natural latex, stir well and evenly, then add 70 parts of natural latex, stir well and evenly to obtain a latex mixture. Then add 37 parts of soaked clay to the mixture, wash the soaked clay residue twice with 5 parts of soft water on the mixing barrel wall soaked with clay and add it to the latex mixture, add 0.5 parts of black slurry, stir until the material is well and evenly. The black scraping cloth slurry for the anti-static rubber shoe sponge midsole cloth is obtained. Store for more than 3 hours and use.
Claims
1. Anti-static rubber shoe sponge midsole cloth black scraper glue, characterized by: The invention is prepared from the following raw materials in parts by weight: 100 parts of natural latex, 15-25 parts of kaolin, 43-45 parts of soft water, 10-14 parts of sodium silicate, 1.0-2.0 parts of mildew preventer BCM, 0.05-0.15 parts of potassium hydroxide, 2.5-3.5 parts of sodium carboxymethyl cellulose, 0.3-0.5 parts of perchlorate, 0.5-1.5 parts of penetrant and 0.4-0.6 parts of black pulp.
2. The anti-static rubber shoe sponge midsole cloth black scraper glue according to claim 1, characterized in that: The invention is prepared from the following raw materials in parts by weight: 100 parts of natural latex, 20 parts of kaolin, 44 parts of soft water, 12 parts of sodium silicate, 1.5 parts of mildew preventer BCM, 0.1 parts of potassium hydroxide, 3 parts of sodium carboxymethyl cellulose, 0.4 parts of perchlorate, 1.0 parts of penetrant and 0.5 parts of black pulp.
3. The anti-static rubber shoe sponge midsole cloth black scraper glue according to claim 1 or 2, characterized in that: The specifications of sodium silicate are: a sodium silicate aqueous solution with a silicon dioxide content ≥24.6% and a Baume degree of 0.35-0.37; the solid content of natural latex is 60%; the specification of sodium carboxymethyl cellulose is FH9; the specification of potassium oxide is industrial grade; the specification of Pingpingjia is type O; the model of the penetrant is JFC; the model of the black paste is 8501 paint black paste.
4. The method for preparing the black scraping cloth mortar for the antistatic rubber shoe sponge midsole cloth according to any one of claims 1 to 3, characterized in that: Take each component according to the above weight parts; S1: preparing cellulose mother liquor: putting 34 / 44 parts of soft water, all the sodium carboxymethyl cellulose, mildew inhibitor BCM, Periga and penetrant into a blender, stirring slowly and adding all the potassium hydroxide, stirring until the sodium carboxymethyl cellulose is evenly dispersed and has no agglomeration to form a thick liquid, thereby obtaining a cellulose mother liquor; S2 scraper glue manufacturing: S2-1 Preparation of impregnated clay: Add all the kaolin, 5 / 44 parts of soft water, and all the sodium carbonate into a mixing barrel and stir until the kaolin is evenly moistened to obtain 37 parts of impregnated clay; S2-2 Preparation of scraper slurry: stir cellulose mother liquor and 10% natural latex in a slurry mixing barrel, stir thoroughly and evenly, then add 20% natural latex, stir thoroughly and evenly, then add the remaining natural latex, stir thoroughly and evenly to obtain a latex mixture; then add impregnated clay to the mixture, wash the impregnated clay residue twice with the remaining soft water on the mixing barrel wall impregnated with clay and add it to the latex mixture, add black slurry, stir until the material is sufficiently uniform, and obtain the black scraper slurry for anti-static rubber shoe sponge midsole cloth.
5. The application method of the black scraper glue for the antistatic rubber shoe sponge midsole cloth as claimed in any one of claims 1 to 3, characterized in that: Within 48 hours after the preparation of the black scraping mortar for the antistatic rubber shoe sponge midsole cloth, evenly scrape a 0.2-0.4 mm thick mortar layer on the rubber shoe midsole cloth, and the coating area is the cloth surface where the rubber shoe midsole cloth is bonded to the rubber.
6. The application method of the black scraper glue for the antistatic rubber shoe sponge midsole cloth according to claim 5 is characterized by: After the preparation of the anti-static rubber shoe sponge midsole cloth and black scraper cloth, the glue should be stored for more than 3 hours before use.
Citation Information
Patent Citations
Latex slurry used on base fabric in rubber shoe and preparation method thereof
CN101781533A
Anti-static water-based cloth coating mucilage in base cloth in sponges in rubber shoes, and preparation method and application thereof
CN103276599A