Rubber and metal bonding method

By coating and vulcanizing the surface of the metal parts multiple times, the problem of unstable bonding between rubber and metal in the prior art under high temperature environment is solved, and stable bonding and corrosion resistance are achieved in 300°C environment, satisfying the satisfaction of High temperature and corrosive environmental requirements for semiconductor manufacturing.

CN118977429AActive Publication Date: 2024-11-19IC SEAL CO LTD

Patent Information

Application Number
CN202411070990.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The prior art cannot effectively bond rubber and metal in high temperature environments, especially at conditions above 300°C, and lacks corrosion resistance, making it difficult to meet the performance requirements of Bonded slit valve door in semiconductor manufacturing.

Method used

By coating the surface of the metal piece with a specific viscosity slurry multiple times and performing primary vulcanization and secondary vulcanization treatments in the vulcanization device, a high temperature and corrosion-resistant rubber and metal bonding assembly is formed.

Benefits of technology

It realizes stable bonding of rubber and metal bonding assembly in an environment of 300°C, has good bonding strength and plasma etching resistance, and meets the requirements of high temperature and corrosion environments in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980864680000111
    Figure BDA0004980864680000111
  • Figure BDA0004980864680000112
    Figure BDA0004980864680000112
  • Figure BDA0004980864680000121
    Figure BDA0004980864680000121
Patent Text Reader

Abstract

The invention relates to the technical field of bonding, in particular to a rubber and metal bonding method. The invention discloses a method for bonding rubber and metal. The method comprises the following steps: S1, coating the surface of a metal piece with adhesive cement; s2, the metal piece with the surface coated with the adhesive cement is attached to rubber, and the metal piece is placed in a vulcanization device to be subjected to primary vulcanization; s3, placing for 20-24 hours at the temperature of 250-290 DEG C, and carrying out secondary vulcanization to obtain a rubber and metal bonding assembly; the viscosity of the mucilage in the step S1 at 25 DEG C is greater than or equal to 500mPa. S. By adopting the rubber and metal bonding method provided by the invention, the bonding use of a rubber and metal bonding assembly in an environment of 300 DEG C can be met. By adopting the rubber and metal bonding method provided by the invention, the rubber and metal bonding assembly can have corrosion resistance of plasma etching resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bonding, and in particular to a method for bonding rubber and metal. Background Art

[0002] In the semiconductor manufacturing process, a high temperature environment is required for processing. High temperature processing helps promote chemical reactions and physical changes in materials, accelerates the reaction speed between materials, and changes the performance and structure of materials, thereby meeting the requirements of advanced processes for material properties; in advanced processes, the structure and function of chips are more complex, and the performance requirements for materials are also higher; through high temperature treatment, defects and impurities in materials can be eliminated, the purity and crystallinity of materials can be improved, thereby enhancing the stability and reliability of materials and ensuring the stability and reliability of chips in long-term operation. In advanced processes, the size and shape of each part of the chip need to be precisely controlled to ensure the performance and stability of the chip. However, in the long run, semiconductor processes face the challenge of higher temperatures. In the semiconductor manufacturing process, equipment often needs to operate at higher temperatures, especially in certain advanced processing steps, such as heat treatment, baking, etc. In the semiconductor manufacturing process, a high degree of cleanliness and vacuum environment need to be maintained to prevent impurities from affecting product quality. Therefore, the vacuum system plays a vital role, and the Bonded slit valve door (BSV) is one of the key components to ensure the normal operation of this system. However, as part of the vacuum system, the Bonded slit valve door includes metal, rubber, and the middle part connecting metal and rubber. It must be able to withstand these high temperature environments without failure, thereby maintaining a high degree of cleanliness and vacuum environment to prevent impurities from affecting product quality. In addition, in addition to high temperature resistance, BSV may also need to meet other performance requirements, such as corrosion resistance and wear resistance, to adapt to the complex process environment and operating requirements in the semiconductor manufacturing process.

[0003] The Chinese patent with patent publication number CN101611064A discloses a method for bonding a perfluoroelastomer material to a surface, but does not provide a solution to the problem of improving the high temperature resistance and corrosion resistance of the adhesive. In addition, the operating environment temperature of the cold adhesive or hot vulcanized adhesive currently on the market is about 230°C, which cannot meet the bonding requirements of the adhesive assembly in an environment of 300°C.

[0004] Therefore, providing a method for bonding rubber and metal with high temperature resistance and corrosion resistance is the main technical problem that needs to be solved at present. Summary of the invention

[0005] In order to solve the above problems, the first aspect of the present invention provides a method for bonding rubber to metal, comprising the following steps:

[0006] S1. Apply glue on the surface of metal parts;

[0007] S2. The metal part coated with glue is bonded to the rubber and placed in a vulcanizing device for primary vulcanization;

[0008] S3. Place at a temperature of 250-290 ° C for 20-24h for secondary vulcanization to obtain a rubber and metal bonding assembly;

[0009] The viscosity of the glue in S1 at 25° C. is ≥500 mPa.s.

[0010] In the present invention, the contact portion between the metal part and the rubber is coated with glue, and a BSV product resistant to 300°C can be obtained through the bonding method provided in the present application, including the bonding portion being able to withstand a high temperature of 300°C.

[0011] In one embodiment, the number of times the glue is applied to the surface of the metal part in S1 is greater than 1.

[0012] In a preferred embodiment, the number of times the glue is applied to the surface of the metal part in S1 is greater than or equal to 2.

[0013] In a more preferred embodiment, the number of times the glue is applied on the surface of the metal part in S1 is 3.

[0014] In one embodiment, after the surface of the metal part in S1 is coated with glue, it is placed at 20-30° C. for 10-15 minutes.

[0015] In one embodiment, the time for which the surface of the metal part is placed at 20-30° C. after the glue is coated on the surface of the metal part in S1 includes but is not limited to 10 min, 11 min, 12 min, 13 min, 14 min, and 15 min.

[0016] In one embodiment, the adhesive is coated on the surface of the metal part 2-3 times, and after the first coating, it is left standing at room temperature for 10-15 minutes, and after the second coating, it is also left standing for 10-15 minutes, and the third coating is consistent with the previous two coating processes.

[0017] In one embodiment, the metal part surface in S1 is allowed to stand at 25°C for 15 minutes after the first coating of glue, and is also allowed to stand at 25°C for 15 minutes after the second coating of glue, and is allowed to stand at 25°C for 15 minutes after the third coating of glue.

[0018] In a preferred embodiment, the surface of the metal part in S1 is coated with glue and then placed at 25°C.

[0019] In one embodiment, the temperature for vulcanization in S2 is 160-180° C., and the vulcanization time is 10-30 min.

[0020] In a preferred embodiment, the temperature for vulcanization in S2 includes but is not limited to 160°C, 161°C, 162°C, 163°C, 164°C, 165°C, 166°C, 167°C, 168°C, 169°C, 170°C, 171°C, 172°C, 173°C, 174°C, 175°C, 176°C, 177°C, 178°C, 179°C, and 180°C.

[0021] In a preferred embodiment, the time for vulcanization in S2 includes but is not limited to 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min, and 30 min.

[0022] In one embodiment, the viscosity of the glue in S1 at 25° C. is 500-2000 mPa.s.

[0023] In one embodiment, the components of the glue in S1 include: fluororubber, curing agent, and solvent.

[0024] In one embodiment, the weight ratio of the curing agent, fluororubber, and solvent is 1:(80-120):(800-1200).

[0025] In a preferred embodiment, the weight ratio of the curing agent, fluororubber and solvent is 1:100:1000.

[0026] In order to improve the adhesion between rubber and metal parts, and further improve the adhesion at high temperatures, the inventors found during the experiment that by coating the glue on the surface of the metal part more than 1 times, especially when the number of times the glue is coated on the surface of the metal part is 3, and the viscosity of the glue at 25°C is 500-2000mPa.s, the rubber and the metal part can be better bonded after primary vulcanization and secondary vulcanization, which can meet the bonding requirements of the rubber and metal bonding assembly in an environment of 300°C; the possible reason is that after multiple coatings of the glue, the glue can be embedded and connected with the surface of the metal part, so that the glue can not only contact the surface of the metal part, but can further penetrate into the concave surface of the metal part, so that after primary vulcanization and secondary vulcanization, it can be better bonded to the rubber, and has corrosion resistance resistant to plasma etching, so that the rubber and metal bonding assembly can have good bonding strength.

[0027] In one embodiment, the curing agent is a diamine compound.

[0028] In one embodiment, the diamine compound is selected from one or more of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, and 2,2-bis(3-amino-4-hydroxyphenyl)propane.

[0029] In one embodiment, the diamine compound is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.

[0030] In one embodiment, the fluororubber is a triazine system perfluororubber.

[0031] In one embodiment, the triazine system perfluororubber can be purchased under the manufacturer model of Solvay 1055B.

[0032] In one embodiment, the solvent is a fluorinated liquid.

[0033] The model of the fluorinated liquid is FC-84 from 3M.

[0034] In one embodiment, the method for preparing the mortar in S1 comprises the following steps:

[0035] The fluororubber and the curing agent are dissolved in a solvent, and then mixed to obtain a glue paste.

[0036] In one embodiment, the method for preparing the mortar in S1 comprises the following steps:

[0037] C1. dissolving the fluororubber using a portion of the solvent to obtain a first solution;

[0038] C2. using the remaining solvent to dissolve the curing agent to obtain a second solution;

[0039] C3. Mix the first solution and the second solution to obtain slurry.

[0040] The weight ratio of the curing agent, fluororubber and solvent in the mortar is 1:100:1000.

[0041] In the implementation manner, the specific amount of solvent used in the first solution and the second solution is not specifically limited, and is determined by the amount that can fully dissolve the fluororubber or the curing agent during the actual experiment. As long as the amount of solvent that can dissolve the fluororubber or the curing agent is within the technical scope of the present application.

[0042] In one embodiment, the dissolution time of the fluororubber by the solvent is 72-96 hours.

[0043] In one embodiment, the dissolution time of the solvent to dissolve the fluororubber includes but is not limited to 72h, 73h, 74h, 75h, 76h, 77h, 78h, 79h, 80h, 81h, 82h, 83h, 84h, 85h, 86h, 87h, 88h, 89h, 90h, 91h, 92h, 93h, 94h, 95h, and 96h.

[0044] Beneficial Effects

[0045] 1. By adopting the rubber and metal bonding method provided in the present application, the rubber and metal bonding assembly can be bonded in an environment of 300°C.

[0046] 2. By adopting the rubber-metal bonding method provided in the present application, the rubber-metal bonding assembly can be made to have corrosion resistance resistant to plasma etching.

[0047] 3. By adopting the rubber and metal bonding method provided in the present application, the rubber and metal bonding assembly can have good bonding strength.

[0048] 4. By limiting the bonding method between rubber and metal used in this application, rubber and metal parts can be better bonded.

[0049] 5. The bonding method provided in this application can obtain a BSV product that is resistant to 300°C. DETAILED DESCRIPTION

[0050] Example 1

[0051] This embodiment provides a method for bonding rubber to metal, comprising the following steps:

[0052] S1. Apply glue on the surface of metal parts;

[0053] S2. The metal part coated with glue is bonded to the rubber and placed in a vulcanizing device for primary vulcanization;

[0054] S3. Place at a temperature of 270°C for 22 hours for secondary vulcanization to obtain a rubber and metal bonding assembly;

[0055] The number of times the glue is applied on the surface of the metal part in S1 is 3; after the first application of glue on the surface of the metal part in S1, it is left at 25°C for 15 minutes, after the second application of glue, it is also left at 25°C for 15 minutes, and after the third application of glue, it is left at 25°C for 15 minutes.

[0056] The amount of glue applied for the first time, the amount of glue applied for the second time, and the amount of glue applied for the third time are all the same, the thickness of a single coating is 0.05 mm, and the width and length of the adhesive bonding surface are 12.5 mm*25 mm.

[0057] The vulcanization temperature in S2 is 170° C., the vulcanization time is 20 min, and the vulcanization pressure is 15 MPa.

[0058] The components of the glue in S1 include: fluororubber, curing agent, and solvent.

[0059] The fluororubber is a triazine system perfluororubber, and the manufacturer's model that can be purchased is Solvay 1055B.

[0060] The curing agent is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.

[0061] The solvent is a fluorinated liquid, model 3M FC-84.

[0062] The method for preparing the mortar in S1 comprises the following steps:

[0063] C1. dissolving the fluororubber using a portion of the solvent to obtain a first solution;

[0064] C2. using the remaining solvent to dissolve the curing agent to obtain a second solution;

[0065] C3. Mix the first solution and the second solution to obtain slurry.

[0066] The amount of the solvent used in the first solution and the amount of the solvent used in the second solution are calculated based on the amount of the solvent that can completely dissolve the fluororubber and the curing agent.

[0067] The weight ratio of the curing agent, fluororubber and solvent in the mortar is 1:100:100.

[0068] The fluororubber used in C1 is in block shape with a size of 2*2*2mm. 3 .

[0069] The dissolution time of the fluororubber by the solvent is 80 hours.

[0070] Example 2

[0071] This embodiment provides a method for bonding rubber to metal, comprising the following steps:

[0072] S1. Apply glue on the surface of metal parts;

[0073] S2. The metal part coated with glue is bonded to the rubber and placed in a vulcanizing device for primary vulcanization;

[0074] S3. Place at a temperature of 270°C for 22 hours for secondary vulcanization to obtain a rubber and metal bonding assembly;

[0075] The number of times the glue is applied on the surface of the metal part in S1 is 3; after the first application of glue on the surface of the metal part in S1, it is left at 25°C for 15 minutes, after the second application of glue, it is also left at 25°C for 15 minutes, and after the third application of glue, it is left at 25°C for 15 minutes.

[0076] The amount of glue applied for the first time, the amount of glue applied for the second time, and the amount of glue applied for the third time are all the same, the thickness of a single coating is 0.05 mm, and the width and length of the adhesive bonding surface are 12.5 mm*25 mm.

[0077] In S1, the surface of the metal part is coated with glue and then placed at 25°C.

[0078] The vulcanization temperature in S2 is 170° C., the vulcanization time is 20 min, and the vulcanization pressure is 15 MPa.

[0079] The components of the glue in S1 include: fluororubber, curing agent, and solvent.

[0080] The fluororubber is a triazine system perfluororubber, and the manufacturer's model that can be purchased is Solvay 1055B.

[0081] The curing agent is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.

[0082] The solvent is a fluorinated liquid, model 3M FC-84.

[0083] The method for preparing the mortar in S1 comprises the following steps:

[0084] C1. dissolving the fluororubber using a portion of the solvent to obtain a first solution;

[0085] C2. using the remaining solvent to dissolve the curing agent to obtain a second solution;

[0086] C3. Mix the first solution and the second solution to obtain slurry.

[0087] The amount of the solvent used in the first solution and the amount of the solvent used in the second solution are calculated based on the amount of the solvent that can completely dissolve the fluororubber and the curing agent.

[0088] The weight ratio of the curing agent, fluororubber and solvent in the mortar is 1:100:500.

[0089] The fluororubber used in C1 is in block shape with a size of 2*2*2mm. 3 .

[0090] The dissolution time of the fluororubber by the solvent is 80 hours.

[0091] Example 3

[0092] This embodiment provides a method for bonding rubber to metal, comprising the following steps:

[0093] S1. Apply glue on the surface of metal parts;

[0094] S2. The metal part coated with glue is bonded to the rubber and placed in a vulcanizing device for primary vulcanization;

[0095] S3. Place at a temperature of 270°C for 22 hours for secondary vulcanization to obtain a rubber and metal bonding assembly;

[0096] The number of times the glue is applied on the surface of the metal part in S1 is 3; after the first application of glue on the surface of the metal part in S1, it is left at 25°C for 15 minutes, after the second application of glue, it is also left at 25°C for 15 minutes, and after the third application of glue, it is left at 25°C for 15 minutes.

[0097] The amount of glue applied for the first time, the amount of glue applied for the second time, and the amount of glue applied for the third time are all the same, the thickness of a single coating is 0.05 mm, and the width and length of the adhesive bonding surface are 12.5 mm*25 mm.

[0098] In S1, the surface of the metal part is coated with glue and then placed at 25°C.

[0099] The vulcanization temperature in S2 is 170° C., the vulcanization time is 20 min, and the vulcanization pressure is 15 MPa.

[0100] The components of the glue in S1 include: fluororubber, curing agent, and solvent.

[0101] The fluororubber is a triazine system perfluororubber, and the manufacturer's model that can be purchased is Solvay 1055B.

[0102] The curing agent is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.

[0103] The solvent is a fluorinated liquid, model 3M FC-84.

[0104] The method for preparing the mortar in S1 comprises the following steps:

[0105] C1. dissolving the fluororubber using a portion of the solvent to obtain a first solution;

[0106] C2. using the remaining solvent to dissolve the curing agent to obtain a second solution;

[0107] C3. Mix the first solution and the second solution to obtain slurry.

[0108] The amount of the solvent used in the first solution and the amount of the solvent used in the second solution are calculated based on the amount of the solvent that can completely dissolve the fluororubber and the curing agent.

[0109] The weight ratio of the curing agent, fluororubber and solvent in the mortar is 1:100:1000.

[0110] The fluororubber used in C1 is in block shape with a size of 2*2*2mm. 3 .

[0111] The dissolution time of the fluororubber by the solvent is 80 hours.

[0112] Example 4

[0113] This embodiment provides a method for bonding rubber to metal, comprising the following steps:

[0114] S1. Apply glue on the surface of metal parts;

[0115] S2. The metal part coated with glue is bonded to the rubber and placed in a vulcanizing device for primary vulcanization;

[0116] S3. Place at a temperature of 270°C for 22 hours for secondary vulcanization to obtain a rubber and metal bonding assembly;

[0117] The number of times the glue is applied on the surface of the metal part in S1 is 3; after the first application of glue on the surface of the metal part in S1, it is left at 25°C for 15 minutes, after the second application of glue, it is also left at 25°C for 15 minutes, and after the third application of glue, it is left at 25°C for 15 minutes.

[0118] The amount of glue applied for the first time, the amount of glue applied for the second time, and the amount of glue applied for the third time are all the same, the thickness of a single coating is 0.05 mm, and the width and length of the adhesive bonding surface are 12.5 mm*25 mm.

[0119] In S1, the surface of the metal part is coated with glue and then placed at 25°C.

[0120] The vulcanization temperature in S2 is 170° C., the vulcanization time is 20 min, and the vulcanization pressure is 15 MPa.

[0121] The components of the glue in S1 include: fluororubber, curing agent, and solvent.

[0122] The fluororubber is a triazine system perfluororubber, and the manufacturer's model that can be purchased is Solvay 1055B.

[0123] The curing agent is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.

[0124] The solvent is a fluorinated liquid, model 3M FC-84.

[0125] The method for preparing the mortar in S1 comprises the following steps:

[0126] C1. dissolving the fluororubber using a portion of the solvent to obtain a first solution;

[0127] C2. using the remaining solvent to dissolve the curing agent to obtain a second solution;

[0128] C3. Mix the first solution and the second solution to obtain slurry.

[0129] The amount of the solvent used in the first solution and the amount of the solvent used in the second solution are calculated based on the amount of the solvent that can completely dissolve the fluororubber and the curing agent.

[0130] The weight ratio of the curing agent, fluororubber and solvent in the mortar is 1:100:2000.

[0131] The fluororubber used in C1 is in block shape with a size of 2*2*2mm. 3 .

[0132] The dissolution time of the fluororubber by the solvent is 80 hours.

[0133] Example 5

[0134] This embodiment provides a method for bonding rubber to metal, comprising the following steps:

[0135] S1. Apply glue on the surface of metal parts;

[0136] S2. The metal part coated with glue is bonded to the rubber and placed in a vulcanizing device for primary vulcanization;

[0137] S3. Place at a temperature of 270°C for 22h for secondary vulcanization to obtain a rubber and metal bonding assembly;

[0138] The number of times the adhesive is applied to the surface of the metal part in S1 is 1; after the adhesive is applied to the surface of the metal part in S1, the metal part is left to stand at 25° C. for 15 minutes.

[0139] The thickness of the applied glue is 0.05mm, and the width and length of the glue-coated bonding surface are 12.5mm*25mm.

[0140] In S1, the surface of the metal part is coated with glue and then placed at 25°C.

[0141] The vulcanization temperature in S2 is 170° C., the vulcanization time is 20 min, and the vulcanization pressure is 15 MPa.

[0142] The components of the glue in S1 include: fluororubber, curing agent, and solvent.

[0143] The fluororubber is a triazine system perfluororubber, and the manufacturer's model that can be purchased is Solvay 1055B.

[0144] The curing agent is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.

[0145] The solvent is a fluorinated liquid, model 3M FC-84.

[0146] The method for preparing the mortar in S1 comprises the following steps:

[0147] C1. dissolving the fluororubber using a portion of the solvent to obtain a first solution;

[0148] C2. using the remaining solvent to dissolve the curing agent to obtain a second solution;

[0149] C3. Mix the first solution and the second solution to obtain slurry.

[0150] The amount of the solvent used in the first solution and the amount of the solvent used in the second solution are calculated based on the amount of the solvent that can completely dissolve the fluororubber and the curing agent.

[0151] The weight ratio of the curing agent, fluororubber and solvent in the mortar is 1:100:1000.

[0152] The fluororubber used in C1 is in block shape with a size of 2*2*2mm. 3 .

[0153] The dissolution time of the fluororubber by the solvent is 80 hours.

[0154] Example 6

[0155] This embodiment provides a method for bonding rubber to metal, comprising the following steps:

[0156] S1. Apply glue on the surface of metal parts;

[0157] S2. The metal part coated with glue is bonded to the rubber and placed in a vulcanizing device for primary vulcanization;

[0158] S3. Place at a temperature of 270°C for 22 hours for secondary vulcanization to obtain a rubber and metal bonding assembly;

[0159] The number of times the adhesive is applied to the surface of the metal part in S1 is 2; after the adhesive is applied to the surface of the metal part in S1, the metal part is left at 25° C. for 15 minutes; and after the second application of the adhesive, the metal part is also left at 25° C. for 15 minutes.

[0160] In S1, the surface of the metal part is coated with glue and then placed at 25°C.

[0161] The amount of glue applied for the first time and the amount of glue applied for the second time are the same, the thickness of a single coating is 0.05 mm, and the width and length of the adhesive bonding surface are 12.5 mm*25 mm.

[0162] The vulcanization temperature in S2 is 170° C., the vulcanization time is 20 min, and the vulcanization pressure is 15 MPa.

[0163] The components of the glue in S1 include: fluororubber, curing agent, and solvent.

[0164] The fluororubber is a triazine system perfluororubber, and the manufacturer's model that can be purchased is Solvay 1055B.

[0165] The curing agent is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.

[0166] The solvent is a fluorinated liquid, model 3M FC-84.

[0167] The method for preparing the mortar in S1 comprises the following steps:

[0168] C1. dissolving the fluororubber using a portion of the solvent to obtain a first solution;

[0169] C2. using the remaining solvent to dissolve the curing agent to obtain a second solution;

[0170] C3. Mix the first solution and the second solution to obtain slurry.

[0171] The amount of the solvent used in the first solution and the amount of the solvent used in the second solution are calculated based on the amount of the solvent that can completely dissolve the fluororubber and the curing agent.

[0172] The weight ratio of the curing agent, fluororubber and solvent in the mortar is 1:100:1000.

[0173] The fluororubber used in C1 is in block shape with a size of 2*2*2mm. 3 .

[0174] The dissolution time of the fluororubber by the solvent is 80 hours.

[0175] Comparative Example 1

[0176] Comparative Example 1 provides a method for bonding rubber to metal. The specific implementation method is the same as that of Example 3, except that Comparative Example 1 uses 5150 adhesive replaces the glue used in Example 3.

[0177] Comparative Example 2

[0178] Comparative Example 2 provides a method for bonding rubber to metal. The specific implementation method is the same as that of Example 3, except that Comparative Example 2 uses Rohm and Haas MEGUM 3290-1 fluororubber adhesive instead of the glue used in Example 3.

[0179] The metal parts of the rubber and metal bonding assemblies in Examples 1-6 and Comparative Examples 1-2 are made of the same material. During the experiment, the metal parts were made of 6061 aluminum. The surface of the metal parts was sandblasted and then cleaned with acetone. The roughness of the surface of the metal parts was 120.

[0180] The rubber material used in the rubber and metal bonding assembly in Examples 1-6 and Comparative Examples 1-2 is the same, namely, vulcanizable fluororubber.

[0181] Performance Testing

[0182] 1. Viscosity test

[0183] The viscosity of the adhesive provided in Examples 1-6 was tested at 25°C using the adhesive viscosity determination method of GB T 2794-2022. The test results of 100-500 mPa.s were recorded as A, the test results of 500-2000 mPa.s were recorded as B, the test results of 2000-5000 mPa.s were recorded as C, and the test results of 5000-10000 mPa.s were recorded as D. The test results are shown in Table 1.

[0184] 2. Adhesion test

[0185] The rubber and metal bonding methods provided in Examples 1-6 are used to observe whether the bonding state of the metal parts and the rubber will show separation and cracking. For the metal parts and the rubber in the metal bonding assembly that are inseparable, the bonding strength is tested. The test method is: Bonding strength test method: Determine according to GB T13936-1992 vulcanized rubber and metal bonding tensile shear strength determination method.

[0186] 3. High temperature resistance test

[0187] The metal bonding assemblies provided in Example 3 and Comparative Examples 1 and 2 were placed in a high-temperature oven at 230° C. for aging for 72 hours, and their bonding effects were observed to see whether separation and non-stickiness occurred. The test results are shown in Table 2.

[0188] The metal bonding assemblies provided in Example 3 and Comparative Examples 1 and 2 were placed in a high-temperature oven at 300° C. and aged for 72 hours to observe their bonding effect and whether separation and non-stickiness would occur. The test results are shown in Table 2.

[0189] 4. Corrosion resistance test

[0190] Test object: metal bonding assemblies provided in Example 3 and Comparative Examples 1 and 2;

[0191] Test method: plasma (test method see Table 3 below, temperature 100±5℃, time 60±5min); after plasma irradiation treatment, the bonding strength is tested according to the GB / T 13936-1992 test method, and the change rate of bonding strength before and after plasma irradiation is calculated (refer to the following change rate of bonding strength resistant to chemical agents); the test results are shown in Table 4.

[0192]

[0193] Where: Δδ——Change rate of adhesive chemical resistance strength, %;

[0194] ——The arithmetic mean of the strength of the samples after being placed in air;

[0195] ——The arithmetic mean of the strength of the specimens after immersion in chemical reagents.

[0196] Table 1

[0197] Example Viscosity Adhesion Bond strength (MPa) Example 1 D Separation non-stick / Example 2 C Separation non-stick / Example 3 B Bonding 4 Example 4 A One sulfur bonding, two sulfur cracking / Example 5 B Separation non-stick / Example 6 B One sulfur bonding, two sulfur cracking /

[0198] Table 2

[0199]

[0200]

[0201] Table 3

[0202] gas Pressure / Pa Gas flow rate / sccm Power / W <![CDATA[O2]]> 2±0.5 80±2 800 / 100 <![CDATA[CF4]]> 5±0.5 80±2 800 / 100

[0203] Table 4

[0204]

[0205] For the corrosion resistance test, the change rate of the bonding strength before and after plasma irradiation was used as the criterion: A: bonding strength change rate <1%; B: bonding strength change rate (1-10)%; C: bonding strength change rate (10-20)%; D: bonding strength change rate ≥20%.

Claims

1. A method for bonding rubber to metal, characterized in that: The following steps are involved: S1. Apply glue on the surface of metal parts; S2. The metal part coated with glue is bonded to the rubber and placed in a vulcanizing device for primary vulcanization; S3. Place at a temperature of 250-290 ° C for 20-24h for secondary vulcanization to obtain a rubber and metal bonding assembly; The viscosity of the glue in S1 at 25° C. is ≥500 mPa.s.

2. The method for bonding rubber to metal according to claim 1, characterized in that: In S1, the number of times the glue is applied to the surface of the metal part is greater than 1.

3. The method for bonding rubber to metal according to claim 1, characterized in that: In S1, the surface of the metal part is coated with glue and then placed at 20-30°C.

4. The method for bonding rubber to metal according to claim 1, characterized in that: The temperature for vulcanization in S2 is 160-180° C., and the vulcanization time is 10-30 min.

5. The method for bonding rubber to metal according to any one of claims 1 to 4, characterized in that: The viscosity of the glue in S1 at 25° C. is 500-2000 mPa.s.

6. The method for bonding rubber to metal according to claim 1, characterized in that: The components of the glue in S1 include: fluororubber, curing agent, and solvent.

7. The method for bonding rubber to metal according to claim 6, characterized in that: The weight ratio of the curing agent, fluororubber and solvent is 1:(80-120):(800-1200).

8. The method for bonding rubber to metal according to claim 6, characterized in that: The curing agent is a diamine compound.

9. The method for bonding rubber to metal according to claim 1, characterized in that: The method for preparing the mortar in S1 comprises the following steps: The fluororubber and the curing agent are dissolved in a solvent, and then mixed to obtain a glue paste.

10. The method for bonding rubber to metal according to claim 9, characterized in that: The dissolution time of the fluororubber by the solvent is 72-96 hours.

Citation Information

Patent Citations

  • Fluororubber plate cementing, pressurizing and curing method and device

    CN114131940A

  • Producing hybrid component useful for motor vehicle, comprises providing component with breakthrough, applying fiber composite material prefabricated with recess, on component, and pressing component with fiber composite material

    DE102010048399A1

  • Device and method for vulcanizing rubber profiles onto conveyor and process belts

    DE502007006738D1

  • Fluororesin molding, roll and manufacture thereof

    JP1997066570A

  • Laminate for bonding vulcanized fluororubber and vulcanized fluororubber bonding method using it

    JP2006007443A

Cited By

  • Negative-pressure special-shaped rubber metal interface cold bonding method

    CN122401927A