Mixed coating slurry as well as preparation method and application thereof

By using a hybrid coating slurry on the lithium-ion battery separator, including adhesive and supportive polymer microspheres, the problem of cell chip folding is solved, and the performance and safety of lithium-ion batteries are improved.

CN118931271APending Publication Date: 2024-11-12EVE POWER CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411155525.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators are prone to corrodes of the cell chip at high temperatures, resulting in battery deformation, short circuit and safety risks. The high crystallinity and interface resistance of the glued separators limit the performance of lithium-ion batteries.

Method used

The polymer porous base film is coated with a mixed coating slurry, which contains adhesive and supportive polymer microspheres. The component content is adjusted to take into account both insulation and lithium ion conduction properties, and improve the adhesion between the diaphragm and the electrode sheet. Knot force and structural stability.

Benefits of technology

It effectively reduces battery cell deformation, improves the internal resistance, rate performance and cycling performance of lithium-ion batteries, and ensures the dynamics and safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931271A_ABST
    Figure CN118931271A_ABST
Patent Text Reader

Abstract

The invention provides mixed coating slurry as well as a preparation method and application thereof. The mixed coating slurry is prepared from the following components in parts by weight: 1.5 to 3.0 parts of polymer, 3.0 to 7.0 parts of inorganic filler, 0.1 to 2.0 parts of adhesive, 0.1 to 1.5 parts of dispersing agent and 85 to 95 parts of water. According to the invention, the surface of the base membrane is uniformly coated with the mixed coating slurry, so that the wrinkle phenomenon of the lithium ion battery is improved, and the internal resistance, the rate capability, the interface structure and the cycle performance of the lithium ion battery are further optimized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of diaphragm materials, and in particular relates to a mixed coating slurry and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have the characteristics of high specific energy, long cycle life, no memory effect and green environmental protection. The discharge voltage is three times that of nickel-cadmium and nickel-metal hydride batteries. They are widely used in fields such as portable device energy storage batteries and power batteries.

[0003] Among them, the diaphragm is one of the most critical components of lithium-ion batteries. It plays the role of separating electrodes to prevent short circuits, while allowing ions to be freely transmitted through the electrolyte in the membrane pore structure. The performance of the diaphragm directly affects the energy density, power density, cycle life and safety of the battery. At present, the commonly used diaphragms for lithium-ion batteries are mainly polyolefin diaphragms such as polypropylene (PP), polyethylene (PE), PP+ceramic coating, PE+ceramic coating, double-layer PP / PE, double-layer PP / PP and three-layer PP / PE / PP. At present, the field of power batteries mainly uses composite diaphragms with ceramic coatings, which can effectively improve the high-temperature thermal shrinkage effect of polyolefin diaphragms and improve product safety, but often cause serious wrinkles on the interface of the battery cell. The wrinkles will cause the battery to deform, the battery to short-circuit, and the battery capacity to decrease. There is still a safety risk of causing battery explosion.

[0004] In order to ensure the safety of lithium-ion batteries, it is necessary to solve the problem of cell electrode wrinkles from the source. The electrolyte formula can be adjusted to reduce the gas production inside the battery or the expansion of the battery during charging and discharging can be reduced by selecting positive and negative electrode materials with stable material structures. However, with the development of diaphragm modification technology, the glue on the diaphragm is used to stick the electrode and the diaphragm together after the mold is hot-pressed, which improves the hardness of the battery core package, improves the assembly operability, and has good safety performance advantages. It can solve the problem of cell wrinkles more simply and at a lower cost. The current market mainly uses polyvinylidene fluoride (PVDF) double-sided glue-coated diaphragms to improve wrinkles. PVDF has excellent mechanical properties, thermal stability and chemical stability, and is easy to form a film. It has received widespread attention in the field of lithium-ion battery diaphragms. However, PVDF has high crystallinity and large interfacial resistance, which makes it have poor affinity with liquid electrolytes, limiting the application of PVDF in the field of lithium-ion battery diaphragms. In addition, too much glue coating causes poor permeability of the diaphragm, weakens the ability of lithium ions to penetrate, and leads to problems such as reduced battery performance.

[0005] Therefore, it is necessary to propose a method for coating the diaphragm to solve the problem of electrode wrinkles while ensuring the comprehensive performance of lithium-ion batteries. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a mixed coating slurry and a preparation method and application thereof. The present invention improves the wrinkling phenomenon of lithium-ion batteries by uniformly coating the mixed coating slurry on the surface of the base film, and further optimizes the internal resistance, rate performance, interface structure and cycle performance of lithium-ion batteries.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a mixed coating slurry, wherein the mixed coating slurry comprises the following components in parts by weight:

[0009]

[0010] The present invention realizes customized diaphragm functional materials by coating the first coating surface of the polymer porous base film with a functional slurry. The slurry contains adhesive polymer microspheres, which mainly play the role of improving the bonding force between the diaphragm and the pole piece, ensuring that the battery cell does not deform during the cycle; the supporting polymer microspheres play a good supporting role, ensuring that a certain gap can be maintained between the diaphragm and the pole piece after hot pressing of the battery cell, thereby improving the liquid retention performance of the battery cell.

[0011] In addition, the present invention adjusts the content of the above components so that the separator can take into account both insulation and lithium ion conductivity, thereby ensuring that the battery cell has good dynamic performance and safety performance.

[0012] Preferably, the mixed coating slurry comprises the following components in parts by weight:

[0013]

[0014] Preferably, the polymer includes any one of polyvinylidene fluoride, polyurethane, polymethyl methacrylate or polybutyl methacrylate, or a combination of at least two thereof.

[0015] Preferably, the inorganic filler includes any one of boehmite, alumina, barium sulfate or magnesium hydroxide, or a combination of at least two thereof.

[0016] Preferably, the average particle size (D50) of the inorganic filler is 0.1 to 2 μm, for example, 0.1 μm, 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm, etc.

[0017] Preferably, the adhesive comprises any one of styrene-butadiene rubber, polyurethane, epoxy resin or acrylate polymer, or a combination of at least two thereof.

[0018] Preferably, the dispersant includes any one of polyacrylate, polyethylene glycol ether or phosphate compounds, or a combination of at least two thereof.

[0019] Preferably, the mixed coating slurry further comprises a wetting agent.

[0020] Preferably, the wetting agent includes any one of fatty acid polyoxyethylene ether, fluoroalkyl methoxy ether alcohol or fluoroalkyl ethoxy ether alcohol, or a combination of at least two thereof.

[0021] Preferably, the weight portion of the wetting agent in the mixed coating slurry is 0.5 to 1.0 parts, for example, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1.0 parts, etc.

[0022] In a second aspect, the present invention provides a method for preparing the mixed coating slurry according to the first aspect, the method comprising the following steps:

[0023] The polymer, inorganic filler, adhesive, dispersant and water are mixed according to the formula amount to obtain a mixed coating slurry.

[0024] Preferably, the mixed coating slurry further comprises a wetting agent.

[0025] Preferably, the viscosity of the mixed coating slurry is 50-300cp, for example, it can be 50cp, 80cp, 100cp, 150cp, 200cp, 250cp, 300cp, etc.; the solid content is 20-40%, for example, it can be 20%, 25%, 30%, 35%, 40%, etc.

[0026] In a third aspect, the present invention provides a composite diaphragm, comprising a base membrane and a mixed coating disposed on at least one side of the base membrane, wherein the mixed coating is prepared from the mixed coating slurry according to the first aspect.

[0027] Preferably, the thickness of the mixed coating is 7 to 15 μm, for example, 7 μm, 8 μm, 10 μm, 11 μm, 12 μm, 15 μm, etc.

[0028] Preferably, the base film comprises a polyolefin base film, for example, a polyethylene base film or a polypropylene base film.

[0029] In the present invention, the preparation method of the base film includes but is not limited to a wet stretching process.

[0030] Preferably, the base film has a thickness of 5 to 10 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc.

[0031] In the present invention, the composite diaphragm is obtained by coating the mixed coating slurry according to the first aspect onto at least one side of a base film, and then rolling, slitting and packaging are performed in sequence after baking to obtain the composite diaphragm.

[0032] In the present invention, the coating thickness is 2.5 to 3.5 μm, for example, 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm, 3 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm, etc.

[0033] In a fourth aspect, the present invention provides a secondary battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator, wherein the separator is the composite separator according to the third aspect.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention provides a mixed coating slurry, which realizes customized diaphragm functional materials by coating a functional slurry on the first coating surface of a polymer porous base film. The slurry contains adhesive polymer microspheres, which mainly play a role in improving the adhesion between the diaphragm and the pole piece, ensuring that the battery cell does not deform during the cycle process; the supporting polymer microspheres play a good supporting role, ensuring that a certain gap can be maintained between the diaphragm and the pole piece of the battery cell after hot pressing, thereby improving the liquid retention performance of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A schematic diagram of the structure of the composite diaphragm provided for Application Example 1;

[0037] Figure 2 This is the SEM image of the composite diaphragm provided for Application Example 1, with a scale of 1 μm;

[0038] Figure 3 This is the SEM image of the hot-melted rubber particles in the composite diaphragm provided in Application Example 1, with a scale of 1 μm;

[0039] Figure 4 Resistance diagram of a lithium-ion battery provided for Application Example 1;

[0040] Figure 5 The discharge curve of the lithium-ion battery provided for Application Example 1 at -20°C and 1C rate;

[0041] Figure 6 The cycling performance diagram of the lithium-ion battery provided for Application Example 1 at 25°C. DETAILED DESCRIPTION

[0042] The technical solution of the present invention is further described below by combining the accompanying drawings and specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0043] The polyvinylidene fluoride used in the examples and comparative examples of the present invention was purchased from Shandong Deyi New Materials Co., Ltd.; styrene-butadiene rubber was purchased from Shenzhen Haodian Technology Co., Ltd.; polyethylene glycol ether was purchased from Hubei Kewode Chemical Co., Ltd.; and fatty acid polyoxyethylene ether was purchased from Yantai Norda New Materials Technology Co., Ltd.

[0044] Example 1

[0045] This embodiment provides a mixed coating slurry, which includes the following components in parts by weight:

[0046]

[0047] The average particle size of boehmite is 1 μm.

[0048] This embodiment also provides a method for preparing the mixed coating slurry, which comprises the following steps:

[0049] Polyvinylidene fluoride, boehmite, adhesive, dispersant, wetting agent and water are mixed according to the formula amount to obtain a mixed coating slurry.

[0050] Example 2

[0051] This embodiment provides a mixed coating slurry, which includes the following components in parts by weight:

[0052]

[0053] The average particle size of boehmite is 0.1 μm.

[0054] This embodiment also provides a method for preparing the mixed coating slurry, which comprises the following steps:

[0055] Polyvinylidene fluoride, boehmite, adhesive, dispersant, wetting agent and water are mixed according to the formula amount to obtain a mixed coating slurry.

[0056] Example 3

[0057] This embodiment provides a mixed coating slurry, which includes the following components in parts by weight:

[0058]

[0059] The average particle size of boehmite is 2 μm.

[0060] This embodiment also provides a method for preparing the mixed coating slurry, which comprises the following steps:

[0061] Polyvinylidene fluoride, boehmite, adhesive, dispersant, wetting agent and water are mixed according to the formula amount to obtain a mixed coating slurry.

[0062] Example 4

[0063] The difference between this embodiment and embodiment 1 is that the viscosity of the mixed coating slurry is 30cp, and the rest is the same as embodiment 1.

[0064] Example 5

[0065] The difference between this embodiment and embodiment 1 is that the viscosity of the mixed coating slurry is 350cp, and the rest is the same as embodiment 1.

[0066] Comparative Example 1

[0067] The difference between this comparative example and Example 1 is that, in terms of weight percentage, the weight percentage of polyvinylidene fluoride in the mixed coating slurry is 0.5 part, and the weight percentage of boehmite is 1.0 part, and the rest is the same as Example 1.

[0068] Comparative Example 2

[0069] The difference between this comparative example and Example 1 is that, in terms of weight percentage, the weight percentage of polyvinylidene fluoride in the mixed coating slurry is 6 parts, and the weight percentage of boehmite is 10 parts, and the rest is the same as Example 1.

[0070] Application Examples 1 to 5 and Comparative Application Examples 1 to 2

[0071] The mixed coating slurries provided in Examples 1 to 5 and Comparative Examples 1 to 2 are used to prepare a diaphragm, and then assembled to obtain a lithium-ion battery. The preparation method is as follows:

[0072] Preparation of positive electrode sheet: positive electrode active material lithium iron phosphate, conductive carbon black, carbon nanotubes, polyvinylidene fluoride and vapor-grown carbon fiber reinforcement are mixed in a mass ratio of 97.4:0.45:0.25:1.7:0.2 to prepare positive electrode slurry, the positive electrode slurry is coated on the surface of aluminum foil, and the positive electrode sheet is obtained after drying;

[0073] Preparation of negative electrode sheet: Graphite, conductive carbon black, sodium carboxymethyl cellulose and styrene-butadiene rubber are mixed in a mass ratio of 96.7:0.6:1.2:1.5 to prepare negative electrode slurry, the negative electrode slurry is coated on the surface of copper foil, and the negative electrode sheet is obtained after drying;

[0074] Preparation of lithium-ion batteries: Assemble the positive electrode sheet, negative electrode sheet, separator and electrolyte to obtain a lithium-ion battery.

[0075] Test conditions

[0076] The lithium-ion batteries provided in Application Examples 1 to 5 and Comparative Application Examples 1 to 2 were tested, and the testing method was as follows:

[0077] (1) DC resistance (DCR) at different states of charge:

[0078] At 25°C, charge the battery to 3.65V at a constant current of 0.33C, switch to constant voltage charging, and cut off when the current reaches 0.05C (9.4A). After leaving it for 1h, discharge it at 0.33C for 0.05Q (Q is the initial capacity of the battery), leave it for 30min, record the voltage at this time as V0, discharge it at 1C for 30s, record the discharge amount as Q', record the voltage at this time as V1, and the DCR at this SOC = (V1-V0) / 1C. Charge Q' back to the battery at 0.33C, repeat the above steps, and measure the DCR at other SOCs.

[0079] (2) Rate performance:

[0080] At 25°C, the battery was charged to 3.65V at a constant current of 0.33C (62.7A), then switched to constant voltage charging and the current was cut off when it reached 0.05C (9.4A). After standing for 1h, it was discharged to 2.0V at 1C at -20°C.

[0081] (3) Cycle performance:

[0082] The charge and discharge test was carried out at a temperature of 25±3℃. The charging method was 3C constant current charging to 3.65V, then switching to constant voltage charging with a cutoff of 0.05C. The discharge method was 1C discharge to 2.5V.

[0083] from Figure 1-Figure 3 It can be seen that the surface of the diaphragm prepared in Application Example 1 is relatively flat and dense, and has good structural stability at high temperatures. Figure 4 It can be seen that the DC resistance of the lithium-ion battery provided in Application Example 1 is small; Figure 5-Figure 6 It can be seen that the lithium-ion battery provided in Application Example 1 has good discharge performance at -20°C and 1C rate, and has a long cycle life at 25°C.

[0084] In summary, the present invention regulates the specific composition of the mixed coating slurry, as well as the parameters of the mixed coating slurry, such as viscosity, so that the prepared mixed coating and the base film have good adhesion and structural stability, thereby ultimately improving the insulation and lithium ion conductivity of the diaphragm, thereby ensuring that the battery cell has good dynamic performance and safety performance.

[0085] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A mixed coating slurry, characterized in that: The mixed coating slurry comprises the following components in parts by weight:

2. The mixed coating slurry according to claim 1, characterized in that: The mixed coating slurry comprises the following components in parts by weight:

3. The mixed coating slurry according to claim 1 or 2, characterized in that: The polymer includes any one of polyvinylidene fluoride, polyurethane, polymethyl methacrylate or polybutyl methacrylate, or a combination of at least two thereof.

4. The mixed coating slurry according to any one of claims 1 to 3, characterized in that: The inorganic filler includes any one or a combination of at least two of boehmite, alumina, barium sulfate or magnesium hydroxide; Preferably, the average particle size of the inorganic filler is 0.1-2 μm.

5. The mixed coating slurry according to any one of claims 1 to 4, characterized in that: The adhesive comprises any one or a combination of at least two of styrene-butadiene rubber, polyurethane, epoxy resin or acrylate polymer; Preferably, the dispersant comprises any one or a combination of at least two of polyacrylate, polyethylene glycol ether or phosphate compounds; Preferably, the mixed coating slurry further comprises a wetting agent; Preferably, the wetting agent comprises any one or a combination of at least two of fatty acid polyoxyethylene ether, fluoroalkyl methoxy ether alcohol or fluoroalkyl ethoxy ether alcohol; Preferably, the weight portion of the wetting agent in the mixed coating slurry is 0.5 to 1.0 parts by weight.

6. A method for preparing a mixed coating slurry according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: The polymer, inorganic filler, adhesive, dispersant and water are mixed according to the formula amount to obtain a mixed coating slurry.

7. The method according to claim 6, characterized in that The mixed coating slurry also includes a wetting agent; Preferably, the viscosity of the mixed coating slurry is 50-300 cp and the solid content is 20-40%.

8. A composite diaphragm, characterized in that: The composite diaphragm comprises a base membrane and a mixed coating disposed on at least one side of the base membrane, wherein the mixed coating is prepared from the mixed coating slurry according to any one of claims 1-5.

9. The composite diaphragm according to claim 8, characterized in that: The thickness of the mixed coating is 7 to 15 μm; Preferably, the base film comprises a polyolefin base film; Preferably, the base film has a thickness of 5 to 10 μm.

10. A secondary battery, characterized in that: The secondary battery comprises a positive electrode, a negative electrode, an electrolyte and a separator, and the separator is the composite separator according to claim 8 or 9.

Citation Information

Patent Citations

  • Composite diaphragm and method for preparing same

    CN103515564A

  • Isolating membrane for lithium ion secondary battery

    CN104953070A

  • Lithium ion battery composite membrane and preparation method thereof

    CN105958000A

  • PVDF (polyvinylidene fluoride) mixed coating diaphragm with good safety and preparation method thereof

    CN106684296A

  • Battery diaphragm and preparation method thereof

    CN108807803A