High-sealing-property wood primer and preparation method thereof

By combining modified acrylic resin and dehydrating agents and other components, the problem of slow coating and poor water vapor penetration caused by wood water absorption in wood sealing primer is solved, and the water resistance of high-enclosed wood primer is achieved and The sealing effect avoids the tendons and color changes on the surface of the wood and extends the service life.

CN118931284APending Publication Date: 2024-11-12GUANGDONG RONGZHIBANG NEW MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411206129.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the use of existing wood sealing primer, the wood absorbs water, causes the coating to dry slowly, and has poor water vapor penetration resistance, resulting in the surface of the wood being easily bulged, and colored components penetrate into the topcoat layer, resulting in yellowing, discoloration, whitening or delamination. Phenomenon.

Method used

Use the combination of modified acrylic resin, dehydrating agent, curing agent, leveling agent, wetting agent, cosolvent and pH adjusting agent to form a highly enclosed wood primer, and modify the acrylic resin and tannin in wood. Acids and other substances form ionic bonds, curing agents promote cross-linking reactions, dehydrating agents reduce moisture, leveling agents improve coating smoothness, assist solvents regulate viscosity, pH adjusters ensure stability, and defoaming agents remove bubbles.

Benefits of technology

It improves the water resistance and sealing properties of the wood primer, reduces the tendon phenomenon caused by the wood's water absorption, prevents the penetration of colored components, extends the service life of the wood, and ensures the uniformity of the coating and appearance quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and particularly relates to a high-sealing-property wood primer and a preparation method thereof. The woodware primer with high sealing property is prepared from the following components in parts by mass: 30 to 50 parts of modified acrylic resin, 3 to 5 parts of a dehydrating agent, 5 to 10 parts of a curing agent, 0.5 to 1.5 parts of a flatting agent, 3 to 6 parts of a wetting agent, 30 to 40 parts of a cosolvent, 0.5 to 1 part of a pH regulator and 0.2 to 0.5 part of a de-foaming agent. The modified acrylic resin and the dehydrating agent are introduced, the crosslinking effect of the modified acrylic resin is utilized to further improve the water resistance and the sealing property of the wood primer, and the dehydrating agent can reduce the water content of the wood primer, so that the water absorption condition of wood in the construction process is reduced; the woodware primer disclosed by the invention can be used for improving the swelling resistance and the sealing effect of woodware, avoiding the situation that colored components of wood permeate into a finishing coat layer through the primer to cause yellowing, discoloring and whitening of the appearance of the woodware, and further prolonging the use experience of the woodware.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a high-sealing wood primer and a preparation method thereof. Background Art

[0002] One of the characteristics of wood is that it expands when it absorbs water and shrinks when it loses water. This is because the cellulose in the wood is hydrophilic, and the colored components in it are also hydrophilic and can dissolve in water.

[0003] Wood sealing primer is a coating used for wood surface treatment. Its main purpose is to provide a protective film for the wood before applying the topcoat to prevent moisture, grease or other impurities inside the wood from penetrating into the topcoat layer, thereby affecting the final coating effect.

[0004] Although the current wood sealing primer can form a protective film after drying, the wood absorbs water during coating, the coating is slow to dry, the water vapor penetration resistance is slow to build, and the resistance to swelling is poor. After the wood is used for a period of time, the wood surface is prone to swelling, and the colored components will penetrate through the primer into the topcoat layer, causing the appearance of the wood to turn yellow, white, or even delaminate. Therefore, it is necessary to develop a highly sealed wood primer to cope with the sealing effect of the coating process on the wood and reduce the appearance of defects in the wood. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of existing wooden articles that after a period of use, the wood surface is prone to bulging, and the colored components will penetrate into the topcoat layer through the primer, causing the appearance of the wooden articles to turn yellow, white, or even delamination, and to provide a highly closed wood primer.

[0006] The present invention adopts the following technical solutions: A high-sealing wood primer comprises the following components in parts by mass: 30-50 parts of modified acrylic resin, 3-5 parts of dehydrating agent, 5-10 parts of curing agent, 0.5-1.5 parts of leveling agent, 3-6 parts of wetting agent, 30-40 parts of cosolvent, 0.5-1 parts of pH regulator and 0.2-0.5 parts of defoaming agent.

[0007] Specifically, acrylic resin has good adhesion, weather resistance and film-forming properties. The modified acrylic resin has higher water resistance and sealing properties than ordinary acrylic resin, and can form a solid and continuous film, effectively sealing the wood surface to prevent moisture and colored components from penetrating, thereby forming a dense protective film. Specifically, the dehydrating agent helps to remove moisture from the coating, promotes better bonding between the primer and the wood, and thus reduces coating problems caused by moisture. Additionally, the curing agent can promote the cross-linking reaction between resin molecules during the drying process of the coating, form a stable coating structure, and improve the hardness and water resistance of the coating. Furthermore, the use of a leveling agent can improve the leveling of the coating, make the coating surface smoother and flatter, and reduce pinholes and orange peel phenomena. The wetting agent helps the coating to better wet the wood surface and improve the adhesion and uniformity of the coating. Further, the cosolvent used in the present invention is used to adjust the viscosity and fluidity of the coating, ensure that the coating is easy to construct and can be evenly coated on the wood surface, and its water content is low, which can reduce the amount of dehydrating agent used. Additionally, the pH regulator of the present invention is used to adjust the pH value of the coating to ensure the stability and coating effect of the coating. The defoamer used in the present invention is used to eliminate bubbles generated during the stirring and construction process of the coating to prevent defects from occurring on the coating surface.

[0008] Tannic acid in wood has hydroxyl groups and good compatibility with water. After wood is painted, tannic acid easily migrates into the paint film. When tannic acid is exposed to air, especially under ultraviolet rays, it is easy to undergo oxidation reaction, which will cause the coating surface to form a yellow or brown quinone structure, thus causing yellowing. At the same time, for coniferous species such as pine, they contain a high content of rosin, which is easy to overflow and penetrate into the paint film, affecting the adhesion and appearance of the paint film. Oils and fats usually contain unsaturated fatty acids and other organic substances, which will gradually oxidize when exposed to air. During this auto-oxidation process, oils and fats will produce free radicals, which will then form chromophores, causing the coating to gradually yellow. Oils and fats will accumulate under the coating, causing bubbles or peeling of the coating over time.

[0009] After the modified acrylic resin of the present invention contacts wood, it can form ionic bonds with molecules of substances such as tannic acid and unsaturated fatty acids in the wood. The salt substances formed by the reaction can fix some substances that easily cause yellowing of the paint film surface on the interface by the coating, and will not migrate and seep out under high temperature and high humidity conditions, and will not be oxidized and discolored on the coating surface, thereby affecting the appearance of the coating. In addition, the dehydrating agent of the present invention can reduce the entry of water into the wood, and can effectively reduce the performance of tannic acid migrating to the paint film along with water. Moreover, the primer of the present invention has a high degree of cross-linking, which forms a blockage to a certain extent and can reduce the tendency of grease overflow.

[0010] A highly closed wood primer, wherein the modified acrylic resin is a cationic acrylic resin. Specifically, the cationic acrylic resin has good adhesion and can firmly adhere to the surface of wood to form a stable protective film. Due to the presence of cationic groups, the modified acrylic resin has good water resistance and can effectively prevent water from penetrating into the interior of the wood, thereby reducing the swelling of the wood due to water absorption.

[0011] Compared with ordinary acrylic resin, cationic acrylic resin has a tighter molecular structure, which helps to form a dense protective film, improve the sealing of the primer, and prevent the colored components and other impurities inside the wood from penetrating into the topcoat layer. Under the action of the curing agent, cationic acrylic resin can undergo a cross-linking reaction to form a three-dimensional network structure, further improving the hardness and weather resistance of the coating.

[0012] A highly closed wood primer, wherein the dehydrating agent is p-toluenesulfonyl isocyanate. In a weakly acidic or acidic environment, the hydroxyl concentration in water is greater than the concentration of the hydroxyl-containing substance in the modified acrylic resin, and p-toluenesulfonyl isocyanate can first react with water to generate carbon dioxide and toluenesulfonamide. After the water is basically reacted, the isocyanate group of p-toluenesulfonyl isocyanate can react with the hydroxyl-containing substance to generate urea and p-toluenesulfonic acid. P-toluenesulfonyl isocyanate can effectively reduce the moisture in the coating, and can reduce the gloss loss, yellowing and reaction foam caused by the wet surface. In the highly closed wood primer, p-toluenesulfonyl isocyanate helps to improve the drying speed and water resistance of the primer, thereby enhancing the sealing effect of the primer on the wood.

[0013] Specifically, dehydrating agents help to enhance the contact between the primer and the wood surface, improve the adhesion of the coating, reduce moisture interference during the drying process of the coating, and reduce defects caused by moisture during coating, such as bubbles and peeling, thereby accelerating the curing and drying of the coating. The coating operation can be completed in a shorter time, improving the overall construction efficiency. The wood surface can better receive the coating, making the coating more uniform and smooth, improving the final appearance and performance, and making the wood products more durable.

[0014] A highly closed wood primer, wherein the curing agent is two or more of 3-aminopropyltriethoxysilane, gamma-methacryloxypropyltrimethoxysilane and aliphatic polyisocyanate.

[0015] Specifically, 3-aminopropyltriethoxysilane has excellent adhesion-promoting properties and a certain waterproof effect. It can form a layer of silicon-oxygen bonds on the surface of wood, enhancing the bonding between the coating and the wood. 3-aminopropyltriethoxysilane also has good reactivity, and its amino functional group can react with a variety of resins and coating components to form stable chemical bonds, further enhancing the network structure of the coating. For example, 3-aminopropyltriethoxysilane can form a covalent bond with the hydroxyl group on the surface of wood, while the amino group at the other end can form a hydrogen bond or a covalent bond with an organic material, thereby improving the mechanical properties and water resistance of the composite material.

[0016] Specifically, γ-methacryloxypropyltrimethoxysilane contains polymerizable methacryloxy groups and silane groups. γ-methacryloxypropyltrimethoxysilane can participate in polymerization under the initiation of free radicals to form a polymer network with excellent weather resistance and water resistance. In wood primers, γ-methacryloxypropyltrimethoxysilane can copolymerize with components such as modified acrylic resins to improve the crosslinking density and chemical resistance of the coating.

[0017] The silane groups of 3-aminopropyltriethoxysilane and γ-methacryloxypropyltrimethoxysilane help to enhance the adhesion between the coating and the wood and improve the overall stability of the coating.

[0018] Specifically, the aliphatic polyisocyanate is a hexamethylene diisocyanate-based isocyanate of Wanhua HT-100, which has excellent hardness and wear resistance, and can react with compounds containing active hydrogen such as hydroxyl and amino groups to form a strong coating. In wood primers, the isocyanate group of the aliphatic polyisocyanate can undergo a cross-linking reaction with the hydroxyl and carboxyl functional groups of components such as modified acrylic resins, significantly improving the hardness and weather resistance of the coating. In addition, compared with aromatic polyisocyanates, aliphatic polyisocyanates have lower yellowing and better environmental protection, reduce VOC emissions, and meet environmental protection requirements.

[0019] The cross-linking reaction of γ-methacryloxypropyltrimethoxysilane and aliphatic polyisocyanate can form a dense polymer network and improve the weather resistance and water resistance of the coating.

[0020] A highly closed wood primer, wherein the cosolvent comprises one or more of dipropylene glycol methyl ether, propylene glycol diacetate, and diethylene glycol butyl ether; Specifically, dipropylene glycol methyl ether has good solubility and volatility, is helpful for dissolving resin and other solid components, has a low volatilization rate, and can improve the fluidity of the coating and reduce brush marks. Specifically, the hydroxyl functional group of dipropylene glycol methyl ether is not as easy to be nucleophilically attacked as the hydroxyl group in alcohol or phenol, and the hydroxyl functional group of dipropylene glycol methyl ether is shielded by the adjacent ether group, thereby reducing the nucleophilicity of the hydroxyl group, and the hydroxyl functional group of dipropylene glycol methyl ether is not sufficient to react effectively with toluenesulfonyl isocyanate.

[0021] Propylene glycol diacetate has low toxicity and good environmental performance. It has high solubility and can effectively dissolve the resin in the coating, increase the fluidity and wettability of the coating, help improve the uniformity of the coating, and stabilize the coating quality. Specifically, the propylene glycol diacetate molecule does not contain free hydroxyl groups, but contains two ester groups. Propylene glycol diacetate is not sufficient to react effectively with toluenesulfonyl isocyanate, so it can reduce the reaction between the dehydrating agent and the cosolvent.

[0022] Butyl diglycol has excellent solubility and wettability, which can help the coating to better wet the wood surface, help reduce foam and improve the drying speed of the coating film, and improve the uniformity of the coating. Specifically, butyl diglycol contains two ether bonds, and the ether groups around the hydroxyl group produce a steric hindrance effect, which reduces the effective contact area between the hydroxyl group and the isocyanate group, thereby reducing the possibility of reaction.

[0023] The reason why wood swells after absorbing water is that the cellulose and hemicellulose components in the wood swell after absorbing water. Wood is composed of cell walls, which are mainly composed of cellulose, hemicellulose and lignin. The looser the wood, the less oil it contains, and the smaller its specific gravity, the stronger its water absorption and the more likely it is to swell. When wood comes into contact with water, cellulose and hemicellulose absorb water, causing the cell wall to swell along the length of the cell wall.

[0024] The solvent of the present invention generally has a small swelling effect on wood. After the wood is treated with the solvent in a dry environment, the moisture content of the wood will be reduced, thereby reducing the possibility of water absorption. The penetration and volatilization process of the solvent in the wood is relatively fast, and it will not form a continuous swelling pressure inside the wood like water.

[0025] The leveling agent is polyether-modified polydimethylsiloxane and polyether siloxane copolymer; specifically, the polyether-modified polydimethylsiloxane of the present invention adopts BYK3700 produced by BYK, and the polyether-modified polydimethylsiloxane can reduce surface tension, optimize the leveling and smoothness of the coating, and reduce coating defects such as pinholes and orange peel; the polyether siloxane copolymer of the present invention adopts Evonik airase5600, and the polyether siloxane copolymer can provide excellent anti-shrinkage and leveling effects, reduce defects on the coating surface, and provide long-term defoaming effect and anti-scratch performance.

[0026] The wetting agent includes one or more of a silicone twin structure surfactant and an acetylene glycol ethoxylate compound; specifically, the silicone twin structure surfactant of the present invention adopts Digo 4100 wetting agent, and the silicone twin structure surfactant can improve the wettability of the coating to the wood and ensure uniform coverage of the coating. Specifically, the acetylene glycol ethoxylate compound of the present invention adopts Evonik 604 wetting agent. The acetylene glycol ethoxylate compound serves as a wetting agent and a leveling agent, and can enhance the uniformity and adhesion of the coating.

[0027] The pH adjuster includes two of sodium hydroxide, sodium carbonate, citric acid and acetic acid; Sodium hydroxide can adjust and increase the pH value of the coating, stabilize the coating performance, and prevent coating defects caused by improper pH. Sodium carbonate is used to fine-tune the pH value and has little effect on the viscosity and stability of the coating. Citric acid and acetic acid can fine-tune the pH value, neutralize excess alkali, keep the coating within the appropriate acid-base range, and optimize the coating curing environment.

[0028] The defoamer includes polyether-modified silicone containing silicon dioxide. Specifically, the polyether-modified silicone containing silicon dioxide of the present invention adopts Deco 920W defoamer. The polyether-modified silicone can effectively eliminate bubbles in the coating and avoid defects such as pinholes and fish eyes in the coating. A highly closed wood primer, the preparation method of the modified acrylic resin, the steps of which include: M1. Acrylic acid, dimethylaminoethyl methacrylate and butyl acrylate are mixed in proportion to form a mixture, and the mixture is slowly added into a reaction kettle while maintaining the reaction temperature; Specifically, acrylic acid, dimethylaminoethyl methacrylate and butyl acrylate are uniformly mixed in a certain proportion to form a reaction monomer mixture. Subsequently, the reaction monomer mixture is slowly added to a reactor while keeping the temperature in the reactor stable. Optionally, the reaction temperature is adjusted to 70° C.-80° C. to maintain a constant temperature.

[0029] M2, the initiator solution is slowly added dropwise into the reactor to initiate the polymerization reaction; Specifically, the initiator azobisisobutyronitrile decomposes at an appropriate temperature to generate free radicals and attack monomer molecules, initiating a chain polymerization reaction to form a high molecular weight acrylic resin. Optionally, the dripping rate is controlled to be completed within 5-10 minutes, the reaction temperature is maintained between 70°C and 80°C, and the reaction is continued for 4 hours.

[0030] M3, slowly add the chain transfer agent solution dropwise into the reactor; Specifically, the chain transfer agent can participate in the polymerization reaction and transfer the active free radicals to the chain transfer agent molecules, thereby controlling the molecular weight distribution of the polymer. The addition of the chain transfer agent dodecanethiol can adjust the branching degree and crosslinking degree of the polymer, reduce the formation of gel, and improve the processing performance and stability of the resin. Optionally, the dripping rate is controlled to be completed within 5-10 minutes. The reaction temperature is maintained between 70°C and 80°C, and the reaction is continued for 2 hours.

[0031] M4. Modified acrylic resin is obtained by concentration, dehydration and purification.

[0032] Specifically, impurities such as unreacted monomers, solvents, oligomers, etc. in the reaction product are removed to improve the purity and performance of the resin.

[0033] Further, the reaction mixture was transferred to a rotary evaporator, and concentrated under reduced pressure to remove the solvent, with the concentration temperature being controlled not to exceed 80°C.

[0034] Further, the concentrated resin is added to a container containing a desiccant, such as molecular sieve or silica gel, to further remove moisture, and placed at room temperature for 24 hours to ensure that the resin is fully dried. The residual desiccant and other impurities are removed by filtration.

[0035] Specifically, acrylic acid contains a large number of carboxyl groups, and the resin contains monomers with tertiary amine groups such as dimethylaminoethyl methacrylate, and these monomers are protonated in subsequent treatments, and the modified resin exhibits certain cationic properties. The prepared modified acrylic resin contains active groups such as carboxyl, hydroxyl, and ester groups.

[0036] A highly closed wood primer, the preparation method of the modified acrylic resin further comprising the following steps: M5. Calculated by mass fraction, 10-20 parts of a cosolvent are added to every 80 parts of the modified acrylic resin, wherein the cosolvent includes one or more of dipropylene glycol methyl ether, propylene glycol diacetate, and diethylene glycol butyl ether. Specifically, after completing the steps of concentration, dehydration, purification, etc., the obtained modified acrylic resin needs to be mixed with a cosolvent to adjust its viscosity and solubility to ensure that the resin can be evenly dispersed in the coating. The cosolvent is slowly added to the modified acrylic resin and fully stirred to ensure that the mixture is uniform, without precipitation and stratification. By adding a cosolvent, the fluidity and wettability of the coating can be improved, thereby optimizing the workability and appearance quality of the coating.

[0037] A highly closed wood primer, the preparation method of the dehydrating agent, the steps comprising: N1, heating benzoic acid and thionyl chloride to generate toluenesulfonyl chloride, and adding a first solvent to obtain a first reaction solution; Specifically, benzoic acid and thionyl chloride are mixed in a certain proportion, heated to an appropriate temperature under reflux conditions, the temperature of the reaction system reaches about 80°C-90°C, and heated for several hours until the reaction is completed. After the reaction is completed, it is cooled to room temperature, and a first solvent is added to dissolve the generated methylbenzenesulfonyl chloride to obtain a first reaction liquid. The first reaction liquid is filtered to remove unreacted solid residues.

[0038] N2, toluene diisocyanate and lysine are reacted, a first catalyst is added, and a second solvent is added to obtain a second reaction solution; Specifically, toluene diisocyanate and lysine are mixed in a certain ratio, toluene diisocyanate and lysine react, slowly heated to about 60°C-70°C, to generate a compound containing an isocyanate group and an amino group, and a first catalyst is added to promote the reaction. Then, a second solvent is added to dissolve the reactants and the generated product to obtain a second reaction liquid, and the second reaction liquid is filtered to remove unreacted solid residues.

[0039] N3, slowly dropwise adding the second reaction liquid into the first reaction liquid, adding the second catalyst and heating for reaction; Specifically, under stirring conditions, the second reaction liquid containing an isocyanate group is slowly added dropwise to the first reaction liquid containing toluenesulfonyl chloride, and the sulfonyl chloride group of toluenesulfonyl chloride reacts with the isocyanate group, and the reaction system is heated under reflux conditions to a temperature of about 80°C-90°C to generate a compound containing a sulfonamide bond, and a second catalyst is added at the same time, and the reaction temperature is controlled within a certain range to accelerate the reaction rate. The heating is continued for several hours until the reaction is completed, and after the reaction is completed, the reaction is cooled to room temperature.

[0040] N4. The reaction product is heated to remove the solvent to obtain a dehydrating agent.

[0041] Specifically, after the reaction is completed, the reaction product is subjected to a heat treatment to remove the solvent therein. The solvent can be removed more effectively by methods such as reduced pressure distillation or atmospheric pressure distillation. After the solvent is removed, the solid or viscous liquid obtained is the desired dehydrating agent. Specifically, the reaction product is transferred to a rotary evaporator to remove the solvent. Concentrate under reduced pressure, and control the concentration temperature not to exceed 80°C.

[0042] A high-sealing wood primer, wherein the first solvent comprises dimethyl sulfoxide or anhydrous chloroform, the second solvent is dimethyl sulfoxide, the first catalyst comprises dimethyl sulfoxide and trimethylamine, and the second catalyst comprises triethylamine or potassium tert-butoxide.

[0043] Specifically, dimethyl sulfoxide has good solubility and good chemical stability, and is not easy to react with reactants. In the process of preparing toluenesulfonyl chloride, dimethyl sulfoxide can be used as a solvent to dissolve benzoic acid and thionyl chloride, as well as the generated toluenesulfonyl chloride.

[0044] In particular, anhydrous chloroform has a lower boiling point and good solubility.

[0045] Specifically, the second solvent is dimethyl sulfoxide. In the reaction of toluene diisocyanate and lysine, dimethyl sulfoxide is used as a solvent to dissolve the reactants and the generated products.

[0046] Specifically, the first catalyst includes dimethyl sulfoxide and trimethylamine. Dimethyl sulfoxide, as a polar solvent and electron donor, participates in the reaction and promotes the activity of the catalyst. In the reaction of toluene diisocyanate and lysine, trimethylamine promotes the reaction between amino groups and isocyanate groups, and accelerates the reaction by neutralizing the acid generated in the reaction or providing an alkaline environment.

[0047] The second catalyst includes triethylamine or potassium tert-butoxide. Specifically, in the reaction of toluenesulfonyl chloride with isocyanate groups, triethylamine can neutralize the acid produced in the reaction, thereby promoting the reaction to proceed in the positive direction. Potassium tert-butoxide can neutralize the acid produced in the reaction and can effectively promote the dehydration reaction.

[0048] A method for preparing a high-sealing wood primer comprises the following steps: S1, adjusting the pH value of the modified acrylic resin to 4.5-6.5, stirring and mixing with a portion of the dehydrating agent, and standing to obtain a first mixed solution; Specifically, the pH value of the modified acrylic resin is adjusted to between 4.5 and 6.5, which can ensure that the resin has stable chemical properties and good compatibility in the subsequent mixing process. The pH value is slightly acidic, which can promote the reaction between the water in the modified acrylic resin and the partial dehydrating agent. The modified acrylic resin with the adjusted pH value is stirred and mixed with the partial dehydrating agent, and the mixture is allowed to stand for a period of time to make the mixture fully uniform to obtain a first mixed solution.

[0049] S2, the first mixed solution is mixed with the remaining dehydrating agent, part of the cosolvent, the leveling agent, the wetting agent, and the defoaming agent, and then stirred, and the mixture is allowed to stand to obtain a second mixed solution, and the pH value of the second mixed solution is adjusted to between 7.5 and 8.5 with a pH adjuster; Specifically, the first mixed solution is mixed with the remaining dehydrating agent, part of the cosolvent, the leveling agent, the wetting agent and the defoamer. The cosolvent helps to adjust the viscosity and ensure the fluidity and uniformity of the mixture. The addition of the leveling agent can improve the surface tension of the coating, making the coating smoother and reducing brush marks and orange peel. The wetting agent can improve the wettability of the coating to the wood surface, ensuring uniform coating coverage without missing or uneven coating. The defoamer is added during the mixing process to eliminate bubbles generated during mixing and avoid defects such as pinholes and fish eyes during coating. The pH value of the second mixed solution is adjusted to 7.5-8.5 with a pH adjuster to maintain the stability and optimal performance of the coating, ensuring that the primer has a suitable pH during subsequent use to avoid adverse effects on wood or other substrates. The addition of these additives can improve the fluidity, wettability and defoaming properties of the primer, thereby improving its construction effect and final quality. The mixture is stirred to ensure that all components are fully mixed and evenly mixed, and left to stand for a period of time to allow the mixture to further stabilize.

[0050] S3, mixing part of the co-solvent with the curing agent to obtain a third mixed solution; Specifically, part of the cosolvent is mixed with the curing agent, the curing agent can initiate a chemical reaction during the drying process of the primer, increase the crosslinking density of the coating, cure the primer and form a hard coating and enhance its chemical resistance, and the addition of the cosolvent helps the curing agent to be evenly dispersed and dissolved in the primer. The mixture is stirred to obtain a third mixed solution, which will be used for subsequent mixing with the second mixed solution.

[0051] S4. Mix the second mixed solution with the third mixed solvent to obtain a highly closed wood primer.

[0052] Specifically, the second mixed solution is mixed with the third mixed solution, and this step is to mix the main components of the primer with the curing agent to form a complete primer formula. The mixture is stirred to ensure that all components are fully mixed and uniform, thereby obtaining a highly closed wood primer. The primer of the present invention has high sealing properties and can effectively prevent external factors such as moisture and stains from penetrating the wood surface, protecting the wood and extending its service life.

[0053] Compared with the prior art, the present invention has the following advantages: 1. The present invention introduces modified acrylic resin and dehydrating agent, and utilizes the cross-linking effect of modified acrylic resin to further improve the water resistance and sealing property of wood primer. The dehydrating agent can reduce the water content of the wood primer itself, thereby reducing the water absorption of wood during the construction process. The wood primer of the present invention can improve the anti-bulking property and sealing effect of wood, and prevent the colored components of wood from penetrating into the topcoat layer through the primer, resulting in yellowing and whitening of the appearance of the wood, thereby further extending the use experience of the wood.

[0054] 2. The preparation process of the present invention is stable and controllable, the preparation process is relatively simple, does not require complex large-scale equipment, and is convenient for large-scale production and application. The prepared wood primer helps to accelerate the establishment of anti-water vapor penetration performance during the wood construction process, can ensure the sealing effect of the wood, and reduce the appearance of defects in the wood. DETAILED DESCRIPTION

[0055] In order to make those skilled in the art more clearly understand the technical solution of the present invention, the following examples are listed for illustration. Unless otherwise specified, the raw materials, reagents or devices used in the following embodiments can be obtained from conventional commercial channels or can be obtained by existing known methods.

[0056] Among them, the aliphatic polyisocyanate is Wanhua HT-100 hexamethylene diisocyanate isocyanate, the polyether modified polydimethyl silicone is BYK3700, the polyether siloxane copolymer is Evonik airase 5600, the silicone twin structure surfactant is Digo 4100 wetting agent, the acetylene glycol ethoxylate is Evonik 604 wetting agent, and the polyether modified silicone of silica is Digo 920W defoamer.

[0057] The present invention will be further described below in conjunction with specific embodiments: Table 1: Mass composition ratio of the formula

[0058] The preparation method of the modified acrylic resin comprises the following steps: M1. Calculated by mass, 30 parts of acrylic acid, 40 parts of dimethylaminoethyl methacrylate and 40 parts of butyl acrylate are mixed in proportion, 50 parts of dimethylformaldehyde are added to form a mixture, the mixture is slowly added to the reactor, and the reaction temperature is adjusted to 70°C-80°C and maintained at a constant temperature.

[0059] M2. Calculate by mass: dissolve 1 part of azobisisobutyronitrile in 10 parts of dichloromethane to form an initiator solution. Add the solution at a rate of 0.1-0.2 parts per minute. Maintain the reaction temperature between 70°C and 80°C and continue the reaction for 4 hours.

[0060] M3. Calculate by mass, dissolve 2 parts of dodecanethiol in 10 parts of dichloromethane to form a chain transfer agent solution, and slowly add it dropwise to the reactor; control the dropwise addition rate to 0.1-0.2 parts per minute. Maintain the reaction temperature between 70°C and 80°C, continue the reaction for 2 hours, and obtain a reaction mixture.

[0061] M4. Transfer the reaction mixture to a rotary evaporator and concentrate to remove the solvent under reduced pressure, controlling the concentration temperature at 70-75°C. Add the concentrated resin to a container containing a silica gel desiccant to further remove moisture, and place it at room temperature for 24 hours to ensure that the resin is fully dried. Remove the residual desiccant and other impurities by filtering to obtain a modified acrylic resin.

[0062] M5. Calculated by mass fraction, 15 parts of cosolvent are added to every 80 parts of modified acrylic resin. The water content of the prepared modified acrylic resin is between 2-4%.

[0063] The preparation method of the dehydrating agent comprises the following steps: N1. 0.5 mol of benzoic acid and excess thionyl chloride are refluxed at a temperature of about 80°C for 3-4 hours until the reaction is completed. Toluenesulfonyl chloride is generated after the reaction is completed. The mixture is cooled to room temperature and 50 ml of anhydrous chloroform is added to dissolve the generated toluenesulfonyl chloride to obtain a first reaction solution. The first reaction solution is filtered to remove unreacted solid residues.

[0064] N2, 0.5 mol toluene diisocyanate and 1 mol lysine are reacted and slowly heated to about 60°C-70°C to generate a compound containing an isocyanate group and an amino group, 0.25% dimethyl sulfoxide and 0.2% trimethylamine are added to the total mass, and 50 ml dimethyl sulfoxide is added to obtain a second reaction liquid; the second reaction liquid is filtered to remove unreacted solid residues.

[0065] N3. Heat under reflux conditions to make the reaction system temperature reach about 80°C-90°C, slowly drop the second reaction liquid into the first reaction liquid, add 0.2% triethylamine by total mass and heat to react; continue heating for 2-4 hours until the reaction is completed. After the reaction is completed, cool to room temperature.

[0066] N4. Concentrate under reduced pressure, control the concentration temperature not to exceed 80° C., and heat the reaction product to remove the solvent to obtain a dehydrating agent.

[0067] A method for preparing a high-sealing wood primer comprises the following steps: S1, adjusting the pH value of the modified acrylic resin to 4.5-6.5, stirring and mixing with a portion of the dehydrating agent, and standing to obtain a first mixed solution; S2, the first mixed solution is mixed with the remaining dehydrating agent, part of the cosolvent, the leveling agent, the wetting agent, and the defoaming agent, and then stirred, and the mixture is allowed to stand to obtain a second mixed solution, and the pH value of the second mixed solution is adjusted to between 7.5 and 8.5 with a pH adjuster; S3, mixing part of the co-solvent with the curing agent to obtain a third mixed solution; S4. Mix the second mixed solution with the third mixed solvent to obtain a highly closed wood primer.

[0068] Example 1 The method for preparing a highly closed wood primer in Example 1 comprises the following steps: S1, adding 15 parts of dipropylene glycol methyl ether to the modified acrylic resin, adjusting the pH value to 4.5, and stirring and mixing with 1.5 parts of a dehydrating agent, the stirring speed is 1200 rpm, the stirring time is 10 min, and after the stirring is completed, the mixture is allowed to stand for 20 hours to obtain a first mixed solution; S2, the first mixed solution is mixed with the remaining dehydrating agent, 10 parts of diethylene glycol butyl ether, a leveling agent, a wetting agent, and a defoaming agent, and then stirred at a stirring speed of 1200 rpm for 20 min. The mixture is allowed to stand for 24 hours to obtain a second mixed solution, and the pH value of the second mixed solution is adjusted to between 7.5 with a pH adjusting agent; the pH adjusting agent is sodium hydroxide and acetic acid; S3, the remaining co-solvent is mixed with the curing agent to obtain a third mixed solution, the stirring speed is 1000 rpm, and the stirring time is 3 min; S4. Stir and mix the second mixed solution and the third mixed solvent for 1 minute to obtain a highly closed wood primer.

[0069] Example 2 The preparation method of a highly closed wood primer in Example 2 comprises the following steps: S1, adding 10 parts of propylene glycol diacetate and 5 parts of dipropylene glycol methyl ether to the modified acrylic resin, adjusting the pH value to 6.5, and stirring and mixing with 2 parts of dehydrating agent, the stirring speed is 1400 rpm, the stirring time is 15min, and after the stirring is completed, the mixture is allowed to stand for 24 hours to obtain a first mixed solution; S2, the first mixed solution and the remaining dehydrating agent, 10 parts of diethylene glycol butyl ether, leveling agent, wetting agent, defoaming agent were mixed and stirred, the stirring speed was 1100 rpm, the stirring time was 15 min, the mixture was allowed to stand for 20 hours to obtain a second mixed solution, and the pH value of the second mixed solution was adjusted to between 8.5 with a pH adjuster; S3, the remaining co-solvent is mixed with the curing agent to obtain a third mixed solution, the stirring speed is 1100 rpm, and the stirring time is 5 min; the pH adjuster is sodium carbonate and citric acid; S4. Stir and mix the second mixed solution and the third mixed solvent for 2 minutes to obtain a highly closed wood primer.

[0070] Example 3 The method for preparing a highly closed wood primer in Example 3 comprises the following steps: S1, adding 15 parts of diethylene glycol butyl ether to the modified acrylic resin, adjusting the pH value to 5.5, and stirring and mixing with 3 parts of a dehydrating agent, the stirring speed is 1600 rpm, the stirring time is 12 min, and after the stirring is completed, the mixture is allowed to stand for 24 hours to obtain a first mixed solution; S2, the first mixed solution is mixed with the remaining dehydrating agent, 10 parts of propylene glycol diacetate, a leveling agent, a wetting agent, and a defoaming agent, and then stirred at a stirring speed of 1200 rpm for 12 min, and the mixture is allowed to stand for 24 hours to obtain a second mixed solution, and the pH value of the second mixed solution is adjusted to between 8.5 with a pH adjuster; the pH adjuster is sodium hydroxide and citric acid; S3, the remaining co-solvent is mixed with the curing agent to obtain a third mixed solution, the stirring speed is 1200 rpm, and the stirring time is 8 min; S4. Stir and mix the second mixed solution and the third mixed solvent for 1 min 30 s to obtain a highly closed wood primer.

[0071] Example 4 The method for preparing a highly closed wood primer in Example 4 comprises the following steps: S1, adding 5 parts of propylene glycol diacetate and 10 parts of dipropylene glycol methyl ether to the modified acrylic resin, adjusting the pH value to 4.5, and stirring and mixing with 2 parts of dehydrating agent, the stirring speed is 1600 rpm, the stirring time is 10min, and after the stirring is completed, the mixture is allowed to stand for 24 hours to obtain a first mixed solution; S2, the first mixed solution and the remaining dehydrating agent, 10 parts of dipropylene glycol methyl ether, leveling agent, wetting agent, defoaming agent are mixed and stirred, the stirring speed is 1200 rpm, the stirring time is 10 min, the mixture is allowed to stand for 24 hours to obtain a second mixed solution, and the pH value of the second mixed solution is adjusted to between 8.0 with a pH adjusting agent; the pH adjusting agent is sodium carbonate and citric acid; S3, the remaining co-solvent is mixed with the curing agent to obtain a third mixed solution, the stirring speed is 1200 rpm, and the stirring time is 8 min; S4. Stir and mix the second mixed solution and the third mixed solvent for 1 minute to obtain a highly closed wood primer.

[0072] Comparative Example 1 The main difference between Comparative Example 1 and Example 4 is that in Comparative Example 1, the modified acrylic resin in Example 4 is replaced with a commercially available hydroxy acrylic resin having a solid content of about 65%, and the other components and operating steps are the same.

[0073] Comparative Example 2 The main difference between Comparative Example 2 and Example 4 is that in Comparative Example 2, p-toluenesulfonyl isocyanate of Example 4 is omitted, and other components and operation steps are the same.

[0074] Comparative Example 3 The main difference between Comparative Example 3 and Example 4 is that the curing agent of Example 4 is omitted in Comparative Example 3, part of the co-solvent of S3 is added to step S2, and the other components and operation steps are the same.

[0075] Comparative Example 4 The main difference between Comparative Example 4 and Example 4 is that the step M5 of modifying the acrylic resin is omitted in Comparative Example 4, that is, 5 parts of propylene glycol diacetate and 10 parts of dipropylene glycol methyl ether are not added, and the cosolvent is added in step S2, and the other components and operation steps are the same.

[0076] Comparative Example 5 The main difference between Comparative Example 5 and Example 4 is that in step S1 of Comparative Example 5, all dehydrating agents are added to the modified acrylic resin, and in step S2, no dehydrating agent is added, and the other components and operation steps are the same.

[0077] Comparative Example 6 The main difference between Comparative Example 6 and Example 4 is that in step S1 of Comparative Example 6, the pH value is not adjusted and the dehydrating agent is not added, and all the dehydrating agent is added in step S2, and the other components and operation steps are the same.

[0078] Comparative Example 7 The main difference between Comparative Example 7 and Example 4 is that in step S1 and step S2 of Comparative Example 7, the mixture is not allowed to stand after stirring and mixing, and the other components and operation steps are the same.

[0079] The above embodiments and comparative examples were subjected to performance tests. The test methods are shown in Tables 2 and 3. After the pine wood was dried, the coating thickness sprayed on the surface of the pine wood was 50 μm. The wood reinforcement test method was to spray water on the primer surface after the primer was completely dried. The spraying amount was 2 ml per 100 g of wood surface. The spraying was performed once every hour. After 5 consecutive sprayings, the wood was stored indoors and the calculation began. After 48 hours, the surface was observed to see if there was reinforcement. The storage temperature was maintained between 25-30 ° C and the humidity was maintained at 100 ° C. Maintain between 40% and 60%, and record the experimental results as no expansion, slight expansion, and severe expansion; among them, the sealing effect test method is that the pine wood surface is first polished with 240# sandpaper, and after the spray-sealed primer is completely dried, it is polished with 400# sandpaper, sprayed with water-based white paint, and kept at room temperature until completely dry. It is first baked in an oven at 60°C for 48 hours, and then stored indoors for 14 days. The storage temperature is maintained between 25-30°C, and the humidity is maintained between 40% and 60%, and the surface is observed for discoloration.

[0080] Table 2: Performance test results of Examples 1-4

[0081] Table 3: Performance test results of comparative examples 1-7

[0082] The preparation process of Examples 1-4 is stable and controllable, the preparation process is relatively simple, does not require complex large-scale equipment, and is convenient for large-scale production and application. The prepared wood primer helps to accelerate the establishment of anti-water vapor penetration performance during the wood construction process, can ensure the sealing effect of the wood, and reduce the appearance of defects in the wood.

[0083] Specifically, the preparation methods of Examples 1-4 can effectively reduce the moisture content of wood primer, so that the coating dries quickly, has fast resistance to water vapor penetration, has good resistance to swelling, and has strong sealing performance.

[0084] In Comparative Example 1, since the modified acrylic resin is replaced with a commercially available hydroxy acrylic resin, the modified acrylic resin in Example 4 is polymerized by acrylic acid, dimethylaminoethyl methacrylate and butyl acrylate, and concentrated, dehydrated and purified to reduce the water content of the modified acrylic resin, so that the water content of the modified acrylic resin can be further reduced by a dehydrating agent in the subsequent stage. The commercially available hydroxy acrylic resin itself can be used in water, so there is no strict requirement for the water content, which results in the hydroxy acrylic resin itself having more water. When a certain amount of p-toluenesulfonyl isocyanate is added, p-toluenesulfonyl isocyanate cannot completely reduce its water content. Therefore, in terms of actual drying time, Example 4 has a shorter actual drying time than Comparative Example 1. In addition, the modified acrylic resin in Example 4 has a high degree of crosslinking, and its performance in polishability, pencil hardness, cross-cut test and yellowing resistance is better than that of Comparative Example 1. The crosslinking density of Comparative Example 1 is poor, resulting in severe bulging. During the subsequent storage process, moisture will slowly precipitate, thereby driving grease or tannic acid to move to the surface of the topcoat to form yellowing.

[0085] In Comparative Example 2, p-toluenesulfonyl isocyanate is omitted. The p-toluenesulfonyl isocyanate in Example 4 can reduce the water content of the wood primer, and the modified acrylic resin in Comparative Example 2 itself has a certain amount of water, which results in that the final water content in Comparative Example 2 is significantly higher than that in Example 4, resulting in a shorter actual drying time in Example 4 than in Comparative Example 2. Since the wood absorbs water during the construction process, water will slowly precipitate during the subsequent storage process, thereby driving grease or tannic acid to move to the surface of the topcoat to form yellowing.

[0086] In Comparative Example 3, the curing agent is omitted, and the cross-linking density of Comparative Example 3 is poor, resulting in severe swelling. In the subsequent storage process, moisture will slowly precipitate, thereby driving grease or tannic acid to move to the surface of the topcoat to form yellowing. The modified acrylic resin in Example 4 has a high degree of cross-linking, and has better performance than Comparative Example 3 in terms of polishability, pencil hardness, cross-cut test and yellowing resistance.

[0087] In Comparative Example 4, no co-solvent is added in step S1, which results in a higher viscosity of the modified acrylic resin itself, making it inconvenient to transfer the modified acrylic resin to a stirring container. During the stirring process, the dehydrating agent is difficult to completely mix with the modified acrylic resin, and the stirring equipment is easily damaged during the preparation process.

[0088] In Comparative Example 5, no dehydrating agent is added in step S2. Although the water content can continue to decrease by continuing to stand for 24 hours in step S2, an excessive amount of dehydrating agent is added in step S1. During the stirring process, the reaction between the dehydrating agent and the modified acrylic resin is relatively violent, resulting in bubbles being easily formed on the surface of the modified acrylic resin without adding a defoaming agent during the stirring process. In Example 4, the gradual addition of the dehydrating agent can better balance the dehydration effect, more finely control the water removal process, and reduce the generation of too many unnecessary bubbles in the first mixed solution during the stirring process.

[0089] In comparative example 6, no dehydrating agent is added in step S1, and the moisture content will not be reduced even if it is left standing. In step S2, on the whole, the standing reaction time of the dehydrating agent and water is correspondingly reduced, and the pH value of the prepared modified acrylic resin is not adjusted. When mixed with other components in step S2, too many components are added at the same time and all dehydrating agents are added at the same time, which will produce a certain violent reaction, resulting in too many unnecessary bubbles in the second mixed solution during the stirring process, local overheating will also cause part of the defoaming agent to precipitate easily due to heat, and insufficient standing time will also cause the final primer to have a slightly higher moisture content, resulting in slight swelling. In the subsequent storage process, moisture will slowly precipitate, thereby driving grease or tannic acid to move to the surface of the topcoat to form yellowing.

[0090] In Comparative Example 7, after the mixing in step S1 and step S2, the mixture is not allowed to stand, resulting in incomplete removal of moisture. The mixture is directly mixed with the curing agent for construction, and the final moisture content of the primer is too high, resulting in severe swelling. During the subsequent storage process, moisture will slowly precipitate, thereby driving grease or tannic acid to move to the surface of the topcoat to form yellowing.

[0091] It can be seen from Table 2 and Table 3 that in Examples 1-4, by introducing modified acrylic resin and dehydrating agent, the cross-linking effect of modified acrylic resin is utilized to further improve the water resistance and sealing property of wood primer. The dehydrating agent can reduce the water content of the wood primer itself, thereby reducing the water absorption of wood during the construction process. The wood primer of Examples 1-4 can improve the anti-bulking property and sealing effect of wood, and prevent the colored components of wood from penetrating into the topcoat layer through the primer, resulting in yellowing and whitening of the appearance of the wood, thereby further extending the use experience of the wood.

[0092] Specifically, the cross-linking strength between the curing agent and the modified acrylic resin used in the wood primer of Examples 1-4 is high, and it is not easy to adhere during sanding in terms of pencil hardness, cross-cut test, yellowing resistance, etc. In addition, its water content is low, which can speed up the actual drying time, reduce the phenomenon of wood rib expansion, and have a good sealing effect.

[0093] The above is a preferred embodiment of the present invention. Relevant personnel in this technical field may make several improvements and modifications without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A highly closed wood primer, characterized in that: The invention comprises the following components in parts by weight: 30-50 parts of modified acrylic resin, 3-5 parts of dehydrating agent, 5-10 parts of curing agent, 0.5-1.5 parts of leveling agent, 3-6 parts of wetting agent, 30-40 parts of auxiliary solvent, 0.5-1 parts of pH adjusting agent and 0.2-0.5 parts of defoaming agent.

2. A highly closed wood primer according to claim 1, characterized in that: The modified acrylic resin is a cationic acrylic resin.

3. The high-sealing wood primer according to claim 1, characterized in that: The dehydrating agent is p-toluenesulfonyl isocyanate.

4. The high-sealing wood primer according to claim 1, characterized in that: The curing agent is two or more of 3-aminopropyl triethoxysilane, γ-methacryloxypropyl trimethoxysilane and aliphatic polyisocyanate.

5. The high-sealing wood primer according to claim 1, characterized in that: The co-solvent includes one or more of dipropylene glycol methyl ether, propylene glycol diacetate, and diethylene glycol butyl ether; the leveling agent is polyether-modified polydimethylsilicon and polyether siloxane copolymer; the wetting agent includes one or more of silicone twin structure surfactants and acetylene glycol ethoxy compounds; the pH adjuster includes two of sodium hydroxide, sodium carbonate, citric acid, and acetic acid; and the defoaming agent includes polyether-modified silicone containing silicon dioxide.

6. The high-sealing wood primer according to claim 1, characterized in that: The preparation method of the modified acrylic resin comprises the following steps: M1. Acrylic acid, dimethylaminoethyl methacrylate and butyl acrylate are mixed in proportion to form a mixture, and the mixture is slowly added into a reaction kettle while maintaining the reaction temperature; M2, the initiator solution is slowly added dropwise into the reactor to initiate the polymerization reaction; M3, slowly add the chain transfer agent solution dropwise into the reactor; M4. Modified acrylic resin is obtained by concentration, dehydration and purification.

7. A highly closed wood primer according to claim 6, characterized in that: The preparation method of the modified acrylic resin further comprises the following steps: M5. Calculated by mass fraction, 10-20 parts of a co-solvent are added to every 80 parts of the modified acrylic resin, wherein the co-solvent includes one or more of dipropylene glycol methyl ether, propylene glycol diacetate, and diethylene glycol butyl ether.

8. The high-sealing wood primer according to claim 1, characterized in that: The preparation method of the dehydrating agent comprises the following steps: N1, heating benzoic acid and thionyl chloride to generate toluenesulfonyl chloride, and adding a first solvent to obtain a first reaction solution; N2, toluene diisocyanate and lysine are reacted, a first catalyst is added, and a second solvent is added to obtain a second reaction solution; N3, slowly dropwise adding the second reaction liquid into the first reaction liquid, adding the second catalyst and heating for reaction; N4. The reaction product is heated to remove the solvent to obtain a dehydrating agent.

9. A highly closed wood primer according to claim 8, characterized in that: The first solvent includes dimethyl sulfoxide or anhydrous chloroform, the second solvent is dimethyl sulfoxide, the first catalyst includes dimethyl sulfoxide and trimethylamine, and the second catalyst includes triethylamine or potassium tert-butoxide.

10. A method for preparing a highly closed wood primer according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1, adjusting the pH value of the modified acrylic resin to 4.5-6.5, stirring and mixing with a portion of the dehydrating agent, and standing to obtain a first mixed solution; S2, the first mixed solution is mixed with the remaining dehydrating agent, part of the cosolvent, the leveling agent, the wetting agent, and the defoaming agent, and then stirred, and the mixture is allowed to stand to obtain a second mixed solution, and the pH value of the second mixed solution is adjusted to between 7.5 and 8.5 with a pH adjuster; S3, mixing part of the co-solvent with the curing agent to obtain a third mixed solution; S4. Mix the second mixed solution with the third mixed solvent to obtain a highly closed wood primer.

Citation Information

Patent Citations

  • Polymethyl methacrylate composite coating and preparation method thereof

    CN102604507A

  • Botton-surface combined type antifouling and antiseptic nanometer polysiloxanes coating and preparation method thereof

    CN106479354A

  • Anti-yellowing furniture paint and preparation method of same

    CN107880682A

  • Novel camouflage painting coating material and preparation method thereof

    CN113248996A

  • Woodware seal primer as well as preparation method and application thereof

    CN113930148A