Preparation method and application of silver coating with MIPs

By combining molecular imprinting technology and surface-enhanced Raman scattering technology, silver coating with MIPs was prepared, which solved the sensitivity and stability of Congo red detection in water, achieved high sensitivity and high selectivity detection effect, and simplified operation The process and shortens the detection time.

CN118931289APending Publication Date: 2024-11-12YANCHENG INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411184056.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, Congo red detection in water bodies has problems such as complex operation, long time consumption, poor sensitivity and poor selectivity, and lacks detection methods with high sensitivity and high selectivity.

Method used

Molecular imprinting technology (MIT) combined with surface-enhanced Raman scattering (SERS) technology was used to prepare silver coatings with MIPs, reduce silver nitrate by ascorbic acid, modify silver nanoparticles, and use Congo red as template and α-methylpropionic acid As functional monomers, Ag@MIPs were prepared by surface blotting method to improve the sensitivity and stability of detection.

Benefits of technology

It significantly improves the sensitivity and stability of Congo red detection, has a short detection time and simple operation, and can detect Congo red at extremely low concentrations, and has good selectivity and reusability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931289A_ABST
    Figure CN118931289A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a silver coating with MIPs, which comprises the following steps: carrying out chemical reduction on silver nitrate by using ascorbic acid as a reducing agent to obtain silver nanoparticles, modifying the silver nanoparticles by using 3-aminopropyltriethoxysilane to obtain Ag-NH2, adding Congo red, alpha-methacrylic acid and Ag-NH2 into a reaction solvent, and reacting at the temperature of 60-80 DEG C to obtain the silver coating with the MIPs. Adding a cross-linking agent after uniformly mixing, adding an initiator after uniformly mixing again, heating and reacting after uniformly mixing, eluting with an eluent after the reaction is finished, and finally drying the precipitate to obtain the product. The silver coating with the MIPs prepared by the method can be used for detection of Congo red, and compared with an existing Congo red detection method, when the silver coating with the MIPs is adopted for detection, the method is easy to operate, the sensitivity and stability of Congo red detection can be remarkably improved, and the detection time is short.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a silver coating with MIPs, belonging to the technical field of chemical detection. Background Art

[0002] Congo red is a water-soluble dye, also known as direct red 28, direct scarlet, cotton red, and direct vermilion. It is a brown-red powder and a red azo dye based on benzidine. Congo red is often used in the clinical diagnosis of amyloid lesions, as a biological stain or acid-base indicator, etc. Congo red can bind to body proteins and is a suspected carcinogen and mutagen. After being absorbed by the human body, under the normal metabolic production reaction conditions of the human body, a reduction reaction may occur to break the azo group and regenerate carcinogenic aromatic amines. After activation, the structure and function of human DNA are changed, causing lesions and inducing cancer. Due to the great harm to human health, it has become a banned azo dye in many countries. At present, my country has paid attention to the supervision of Congo red and has banned Congo red in the textile industry. However, driven by interests, there are still unscrupulous merchants who add such substances to food for coloring. It not only has residues in food, but also easily enters water bodies during production and use, causing harm to the environment. Therefore, it is necessary to detect Congo red in water bodies.

[0003] At present, the detection of Congo red in water bodies generally has the problems of complex operation, long time consumption, poor sensitivity and poor selectivity. Therefore, it is necessary to establish a sensitive, accurate and rapid method for detecting Congo red in water bodies. Surface enhanced Raman scattering (SERS) technology has high sensitivity, simple operation and fast detection speed. It is widely used in the detection of chemical pollutants and has broad development prospects. Molecular imprinting technology (MIT) is a special separation, enrichment and recognition technology used to prepare polymers with specific recognition functions. The polymers obtained by molecular imprinting technology are called molecular imprinted polymers (MIPs), which are artificially synthesized polymers with specific recognition, chemical stability and wide applicability. The combination of molecular imprinting technology (MIT) and surface enhanced Raman scattering (SERS) technology can achieve high-sensitivity and high-selectivity molecular detection. However, there is currently no report on the combination of these two technologies for the detection of Congo red in water bodies.

[0004] Based on this, the inventors prepared a silver coating with MIPs using Congo red as a template molecule and α-methylpropene as a functional monomer, which can significantly improve the sensitivity and stability of Congo red detection. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the Congo red detection method in the prior art and provide a method for preparing a silver coating with MIPs. The prepared silver coating with MIPs can be used for the detection of Congo red, is simple to operate, can significantly improve the sensitivity and stability of Congo red detection, and has a short detection time.

[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0007] A method for preparing a silver coating having MIPs comprises the following steps:

[0008] (1) chemically reducing silver nitrate with ascorbic acid as a reducing agent to obtain silver nanoparticles;

[0009] (2) silver nanoparticles were modified with APTES (3-aminopropyltriethoxysilane) to obtain Ag-NH2;

[0010] (3) Congo red, α-methylacrylic acid and Ag-NH2 are added to a reaction solvent, and a crosslinking agent is added after mixing evenly. An initiator is added after mixing evenly again. After mixing evenly, the reaction is heated and then eluted with an eluent. Finally, the precipitate is dried to obtain a silver coating having MIPs.

[0011] Furthermore, in step (1), the preparation method of the silver nanoparticles is as follows: glutamine is added to the silver nitrate solution, reacted for 10-20 minutes, ascorbic acid is quickly added, stirred for reaction, centrifuged, washed, and dried to obtain the silver nanoparticles.

[0012] Furthermore, in step (2), the preparation method of Ag-NH2 is as follows: silver nanoparticles are added to a mixed solvent consisting of ethanol and deionized water in a volume ratio of 4:1, mixed evenly, and then APTES is added, stirred and reacted at 40°C. After the reaction is completed, centrifugation, washing, and drying are performed to obtain the Ag-NH2.

[0013] Furthermore, in step (3), the molar ratio of Congo red to α-methylacrylic acid is 1:(9-12).

[0014] Furthermore, in step (3), the reaction solvent is any one of acetonitrile, ethanol or toluene, more preferably acetonitrile.

[0015] Furthermore, in step (3), the temperature of the heating reaction is 60° C. and the reaction time is 16-24 hours.

[0016] Furthermore, in step (3), the cross-linking agent is selected from any one of ethylene glycol dimethacrylate (EGDMA), divinylbenzene, glutaraldehyde, epichlorohydrin or N,N'-methylenebisacrylamide.

[0017] Furthermore, in step (3), the initiator is azobisisobutyronitrile (AIBN).

[0018] Furthermore, in step (3), the eluent is a mixture of methanol and acetic acid in a volume ratio of 4:1.

[0019] The silver coating with MIPs prepared by the above method.

[0020] The silver coating with MIPs prepared by the above method is used for detecting Congo red in water.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention provides a method for preparing a silver coating with MIPs, firstly using glutamine as a directing agent and ascorbic acid as a reducing agent, synthesizing silver nanoparticles by chemical reduction method, then modifying the silver nanoparticles by APTES to obtain amino-modified silver nanoparticles, and finally using amino-modified silver as a substrate, methacrylic acid as a functional monomer, and Congo red as a template, preparing Ag@MIPs (silver coating with MIPs) by surface imprinting method. The silver coating with MIPs prepared by the present invention can be used for the detection of Congo red, is simple to operate, can significantly improve the sensitivity and stability of Congo red detection, and has a short detection time. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the SEM image of the Ag@MIPs prepared in Example 1;

[0024] Figure 2 This is the EDS image of Ag@MIPs prepared in Example 1;

[0025] Figure 3 XRD pattern of Ag@MIPs prepared in Example 1;

[0026] Figure 4 FT-IR spectrum of Ag@MIPs prepared in Example 1;

[0027] Figure 5 TGA image of Ag@MIPs prepared in Example 1;

[0028] Figure 6 The SERS spectrum of Ag@MIPs prepared in Example 1;

[0029] Figure 7 The results of detecting Congo red solutions of different concentrations using the silver nanoparticles and Ag@MIPs prepared in Example 1 as SERS substrates;

[0030] Figure 8The selectivity test results of Ag@MIPs prepared in Example 1;

[0031] Fig. 9 This is the SERS spectrum of the Ag@MIPs prepared in Example 1 after being reused three times. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings and specific embodiments.

[0033] Example 1

[0034] A method for preparing a silver coating having MIPs comprises the following steps:

[0035] (1) Silver nitrate was chemically reduced with ascorbic acid as a reducing agent to prepare silver nanoparticles. The specific method was as follows: 0.1698 g of silver nitrate was added to 11.0 mL of deionized water, and after stirring and dissolving, a silver nitrate solution was obtained. 0.1 mL of 0.1 mol L -1 10 mL of glutamine solution was added quickly after reacting for 15 minutes. -1 Ascorbic acid solution was added and stirred for 15 minutes. After the reaction was completed, the mixture was centrifuged and washed with water and ethanol three times respectively. The precipitate was placed in a vacuum drying oven at 60°C and dried for 3 hours to obtain silver nanoparticles.

[0036] (2) Silver nanoparticles were modified with APTES (3-aminopropyltriethoxysilane) to obtain Ag-NH2; the specific method was as follows: 0.1 g of the silver nanoparticles prepared in step (1) was weighed and added into a round-bottom flask, followed by the addition of 32 mL of ethanol and 8 mL of deionized water, which was allowed to stand for 2 minutes to allow the mixture to mix evenly, and then 2 mL of APTES was added. The round-bottom flask was placed in a 40°C oil bath and stirred for 12 hours. After the reaction was completed, the mixture was washed three times by centrifugation with ethanol, the supernatant was poured out, and the solid was dried in a vacuum drying oven at 60°C for 3 hours to obtain the product Ag-NH2.

[0037] (3) 0.1 g of Congo red, 1.0 mL of MAA (α-methyl acrylic acid), and 0.1 g of Ag-NH2 were added to a round-bottom flask containing 27 mL of acetonitrile, and the mixture was ultrasonically mixed for 20 minutes. 1.89 mL of crosslinker EGDMA (ethylene glycol dimethacrylate) was added, and the mixture was ultrasonically mixed for 5 minutes. Then 20 mg of initiator AIBN (azobisisobutyronitrile) was added, and the mixture was ultrasonically mixed for 20 minutes. The mixture was then reacted in an oil bath at 60°C for 16 hours. After the reaction was completed, an eluent was prepared by mixing 200 mL of methanol and 50 mL of acetic acid. The mixture was ultrasonically mixed and shaken until the liquid showed almost no red color. After removing the liquid, the precipitate was dried for 3 hours to obtain a silver coating with MIPs (Ag@MIPs).

[0038] 1. The morphology and elements of the silver nanoparticles and Ag@MIPs prepared in Example 1 were analyzed using a scanning electron microscope and an energy dispersive spectrometer (SEM-EDS, NovaNano SEM 450, FEI).

[0039] Figure 1 This is the SEM image of Ag@MIPs prepared in Example 1, where Figure 1 A is silver nanoparticles, Figure 1 B is Ag@MIPs. It can be seen that the silver nanoparticles are flower-shaped with irregular small particles and a relatively smooth surface. There is no significant difference in the overall shape of Ag@MIPs and silver nanoparticles, but the surface roughness of Ag@MIPs increases. This is because the introduction of the imprinting layer makes their surface rougher.

[0040] Figure 2 This is the EDS image of Ag@MIPs prepared in Example 1, where: Figure 2 A is silver nanoparticles, Figure 2 B is Ag@MIPs. It can be seen that the EDS spectrum of silver nanoparticles shows three elements: Ag, C, and O. Element imaging shows that Ag is the main component with a high overall content, followed by C, and O is the least. After imprinting coating, the EDS spectrum and Ag@MIPs element imaging images show that the content of C and O elements increases, mainly from the imprinting coating, and the increased C and O elements come from functional monomers and crosslinkers. SEM and EDS results show that Ag@MIPs were successfully prepared.

[0041] 2. The crystal structures of the silver nanoparticles and Ag@MIPs prepared in Example 1 were characterized by X-ray diffractometer, and the molecular structure of Ag@MIPs was analyzed by Fourier transform infrared spectrometer.

[0042] Figure 3The XRD pattern of Ag@MIPs prepared in Example 1 shows that there are five characteristic peaks on the XRD spectrum of silver nanoparticles, located at 38.24°, 44.36°, 64.49°, 77.40° and 81.56°, respectively. The above five characteristic peaks correspond to the five crystal planes of the Ag face-centered cubic (fcc) structure, namely (111), (200), (220), (311) and (222). The intensity ratio between the (111) and (200) crystal planes is (3.2) greater than 2.1, indicating that the (111) crystal plane tends to grow along the

[111] direction and has a more advantageous growth. Compared with the XRD spectrum of silver nanoparticles, the XRD spectrum of Ag@MIPs also showed five characteristic peaks, located at 38.12°, 44.26°, 64.39°, 77.41° and 81.56° respectively. The XRD intensity of Ag@MIPs was lower than that of silver nanoparticles, and the position of the characteristic peaks did not change, indicating that the introduction of the imprinting layer had no effect on the crystal phase of the internal Ag particles.

[0043] Figure 4 This is the FT-IR spectrum of Ag@MIPs prepared in Example 1. As shown in the figure, no obvious infrared characteristic peaks of silver nanoparticles were observed, indicating that the unreacted reducing agent and directing agent were washed away by centrifugal washing. Except for the CH vibration peak, there were no other infrared spectrum peaks. However, some characteristic peaks on the infrared spectrum of Ag@MIPs were observed, such as 1384cm -1 -OH bending vibration peak, 1632cm -1 C=O or C=C stretching vibration peak, 2853cm -1 is the CH stretching vibration peak, 2921cm -1 The peak of CH stretching vibration in -CH3 is 3444cm, which is generated by the stretching vibration of -OH. -1 Characteristic peaks. In summary, it is shown that Ag@MIPs are prepared by introducing an imprinting layer on the surface of silver nanoparticles.

[0044] 3. Thermogravimetric analysis of the silver nanoparticles and Ag@MIPs prepared in Example 1 was performed under N2 conditions.

[0045] Figure 5The TGA image of Ag@MIPs prepared in Example 1 shows that the weight loss rate of silver nanoparticles remains within 2% in the temperature range of 30-1000°C; however, the weight loss of Ag@MIPs decreases by about 10% in the temperature range of 200-1000°C, which is due to the loss of the MIPs layer. The thermal analysis chart of Ag@MIPs shows that the weight gradually decreases with increasing temperature, which may be due to the gradual separation of the MIPs layer. The significant reduction in the weight of the first one may be due to the detachment of the MIPs layer. In contrast, the second weight loss is due to the peeling of the silver surface modification layer. The results show that the MIPs layer is successfully coated on the surface of the Ag particles.

[0046] 4. Test the SERS adsorption performance of the silver nanoparticles and Ag@MIPs prepared in Example 1 for Congo red.

[0047] Test method: 20 mg of silver nanoparticles and Ag@MIPs prepared in Example 1 were immersed in 8 mL of 1.0×10 -6 mol / L Congo red solution and placed on an oscillator for 120 min. Then, the experimental samples were transferred to a clean glass slide and allowed to dry naturally before Raman testing.

[0048] Figure 6 The SERS spectrum of Ag@MIPs prepared in Example 1 shows that when silver nanoparticles are used as SERS substrate to detect Congo red, a SERS spectrum with five characteristic peaks is obtained, which are located at 1154 cm -1 、1375cm -1 、1397cm -1 、1449cm -1 and 1594cm -1 . Similar results are also found in related literature. -1 The stretching vibration of -NC- (-N-phenyl) is located at 1375cm -1 .1397cm -1 The stretching vibration of -C-phenyl group. The -N=N- stretching vibration mainly occurs at 1397cm -1 and 1449cm -1 .1594cm -1 In contrast, the SERS substrate obtained by using silver nanoparticles as SERS substrate and Ag@MIPs as SERS substrate is 1287 cm -1There is a characteristic peak at , which is phenyl-phenyl stretching vibration. The adsorption of Congo red functional groups at different positions on the SERS substrate will cause differences in characteristic peaks. Therefore, the SERS characteristic peaks obtained by detecting Congo red on different SERS substrates may have some differences, but they are generally consistent. Therefore, the silver nanoparticles and Ag@MIPs prepared in Example 1 can be used as SERS substrates to realize SERS Congo red detection. Figure 6 It can also be seen that at the same Congo red concentration, the SERS characteristic peak intensity obtained by using Ag@MIPs as a SERS substrate is better than that obtained by using silver nanoparticles as a SERS substrate. This indicates that plasma resonance occurs in the holes of the Ag@MIPs surface imprinting layer, thus providing more "hot spots" for SERS detection.

[0049] 5. The silver nanoparticles and Ag@MIPs prepared in Example 1 were used to detect Congo red solutions of different concentrations.

[0050] Prepare different concentrations (1.0×10 -3 mol L -1 , 1.0×10 -4 mol L -1 , 1.0×10 -5 mol L -1 , 1.0×10 -6 mol L -1 , 1.0×10 -7 mol L -1 ) Congo red solution, 20 mg of silver nanoparticles and Ag@MIPs prepared in Example 1 were immersed in 8 mL of Congo red solution of different concentrations, and placed on an oscillator for 120 min. Subsequently, the experimental samples were transferred to a clean glass slide and allowed to dry naturally for Raman testing.

[0051] Figure 7 The results of the detection of Congo red solutions of different concentrations using the silver nanoparticles and Ag@MIPs prepared in Example 1 as SERS substrates are shown in FIG. Figure 7 A is the detection result of silver nanoparticles as SERS substrate for Congo red solutions of different concentrations. Figure 7 B is the detection result of Ag@MIPs as SERS substrate for Congo red solutions of different concentrations. Figure 7 C is the linear curve of silver nanoparticles detecting different concentrations of Congo red. Figure 7 D is the linear curve of Ag@MIPs detecting different concentrations of Congo red. Figure 7As shown in A, with the increase of Congo red concentration, the characteristic peak intensity obtained by using silver nanoparticles as SERS substrate to detect Congo red gradually increases. By detecting the SERS spectra obtained by different concentrations of Congo red, the same result also appeared in Ag@MIPs ( Figure 7 B). The only difference is that the concentration range of Congo red is 1.0×10 -9 mol L -1 ~1.0×10 -3 mol L -1 The minimum concentration of Congo red detected using Ag@MIPs as SERS substrate is 1.0×10 -9 mol L -1 It is two orders of magnitude lower than the detection result using silver nanoparticles as SERS substrate. -1 、1449cm -1 and 1594cm -1 The characteristic peaks at were linearly fitted ( Figure 7 C and 7D). Silver nanoparticles as SERS substrates detect Congo red in the concentration range of 1.0×10 - 7 mol L -1 ~1.0×10 -3 mol L -1 , at 1154cm -1 The linear fitting of the characteristic peak at 1.0×10 -9 mol L-1~1.0×10 -3 mol L -1 In the concentration range, 1594cm -1 The linear fitting of the characteristic peaks of is the best, and the linear correlation coefficient is 0.9964. In summary, both silver nanoparticles and Ag@MIPs can be used as SERS substrates for the determination of Congo red, and the performance of Ag@MIPs as a SERS substrate is better than that of silver nanoparticles.

[0052] 6. Test the selectivity of Ag@MIPs.

[0053] The MIPs layer with imprinted holes has a specific recognition ability for the template, and the selectivity of Ag@MIPs was studied using methylene blue (MB) as a competitive molecule. -6 mol L -14 mL of each Congo red and methylene blue solution was taken and placed in two centrifuge tubes, and then 20 mg of the Ag@MIPs prepared in Example 1 was added to each of the two centrifuge tubes. The tubes were placed on an oscillator and oscillated for 120 min. Subsequently, the experimental samples were transferred to a clean glass slide and allowed to dry naturally before conducting Raman testing again.

[0054] Figure 8 The selectivity test results of Ag@MIPs prepared in Example 1, where: Figure 8 A is the SERS spectrum of Ag particles detecting Congo red and methylene blue. Figure 8 B is the SERS spectra of Ag@MIPs detecting Congo red and methylene blue. It can be seen that there is no significant difference in the SERS enhancement effect of Ag active substrate on MB and CR, and the enhancement effect on MB is even better than that on CR. Compared with the competing molecule MB, CR shows more effective SERS enhancement performance in Ag@MIPs active substrate.

[0055] 7. Reusability test of Ag@MIPs.

[0056] Test method: 30 mg of Ag@MIPs prepared in Example 1 was added to 6 mL (1.0×10 -7 mol L -1 ) in a Congo red aqueous solution, placed on an oscillator for two hours, and a sample was taken for Raman testing. Then the Ag@MIPs were centrifuged and eluted with an eluent to remove the template molecules. Then the Ag@MIPs were added back to the Congo red aqueous solution and oscillated for two hours, and then a Raman test was performed. After elution with the eluent, they were added back to the Congo red aqueous solution and oscillated for two hours, and then a Raman test was performed.

[0057] Fig. 9 The SERS spectra of the Ag@MIPs prepared in Example 1 after being reused three times show that the intensity of the detected Congo red Raman characteristic peak decreases slightly during the reuse process, but the peak intensity is still significant, which fully demonstrates that the Ag@MIPs can be reused and has good reusability. Due to the excellent reusability of Ag@MIPs, it plays a vital role in detecting organic pollutants in water environments, reducing costs and saving preparation time in practical applications.

Claims

1. A method for preparing a silver coating having MIPs, It is characterized in that The steps include: (1) chemically reducing silver nitrate using ascorbic acid as a reducing agent to obtain silver nanoparticles; (2) Silver nanoparticles were modified with 3-aminopropyltriethoxysilane to obtain Ag-NH 2 ; (3) Congo red, α-methacrylic acid and Ag-NH 2 Add it to the reaction solvent, mix it evenly, then add the crosslinker, mix it evenly again, then add the initiator, mix it evenly, then heat it to react, wash it with the eluent after the reaction is finished, and finally dry the precipitate to obtain a silver coating with MIPs.

2. The method for preparing a silver coating having MIPs as claimed in claim 1, It is characterized in that In step (1), the preparation method of the silver nanoparticles is as follows: glutamine is added to a silver nitrate solution, reacted for 10-20 minutes, ascorbic acid is quickly added, stirred for reaction, centrifuged, washed, and dried to obtain the silver nanoparticles.

3. The method for preparing the silver coating having MIPs as claimed in claim 1, It is characterized in that In step (2), the Ag-NH 2 The preparation method is as follows: silver nanoparticles are added into a mixed solvent consisting of ethanol and deionized water in a volume ratio of 4:1, mixed evenly, and then 3-aminopropyltriethoxysilane is added, and the reaction is stirred at 40°C. After the reaction is completed, the reaction is centrifuged, washed, and dried to obtain the product.

4. The method for preparing a silver coating having MIPs as claimed in claim 1, It is characterized in that In step (3), the molar ratio of Congo red to α-methylacrylic acid is 1:(9-12).

5. The method for preparing the silver coating having MIPs as claimed in claim 1, It is characterized in that In step (3), the reaction solvent is any one of acetonitrile, ethanol or toluene.

6. The method for preparing a silver coating having MIPs as claimed in claim 1, It is characterized in that In step (3), the temperature of the heating reaction is 60° C. and the reaction time is 16-24 hours.

7. The method for preparing a silver coating having MIPs as claimed in claim 1, It is characterized in that In step (3), the cross-linking agent is selected from any one of ethylene glycol dimethacrylate, divinylbenzene, glutaraldehyde, epichlorohydrin or N,N'-methylenebisacrylamide.

8. The method for preparing a silver coating having MIPs as claimed in claim 1, It is characterized in that In step (3), the initiator is azobisisobutyronitrile.

9. A method for preparing a silver coating having MIPs according to any one of claims 1 to 8, It is characterized in that In step (3), the eluent is a mixture of methanol and acetic acid in a volume ratio of 4:

1.

10. Use of the silver coating with MIPs prepared by the method according to any one of claims 1 to 9 in detecting Congo red in water.

Citation Information

Patent Citations

  • Method for preparing surface-enhanced Raman spectroscopy substrate of silver self-assembly under assistance of amino acids

    CN102608099A

  • Method for surface-enhanced Raman scattering spectrum detection by using silver-surface molecularly imprinted polymer

    CN103063649A