Heat-insulating flame-retardant anticorrosive paint and preparation method thereof

By using aluminum powder in the coating, the thermal insulation microcapsules and hollow glass microbeads wrapped in acrylic resin and polyamide resin, combined with epoxy resin, the thermal insulation and flame retardant performance of traditional anticorrosion coatings in high temperature and fire environments is solved. Problem, higher thermal insulation and flame retardant effects are achieved, and the stability and corrosion resistance of the coating are enhanced.

CN118931293AActive Publication Date: 2024-11-12HENAN SUNSHINE ANTICORROSIVE PAINTING CO LTD

Patent Information

Application Number
CN202411233994.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

Traditional anticorrosion coatings have insufficient thermal insulation and flame retardant performance in high temperature and fire environments, and cannot effectively prevent heat transfer and fire spread, increasing safety risks.

Method used

Using thermal insulation flame retardant anti-corrosion coating, the thermal insulation microcapsules formed by adding aluminum powder to the coating are wrapped in acrylic resin and polyamide resin, and combined with hollow glass microbeads and epoxy resin, to form multiple insulation mechanisms to improve the coating. density and flame retardant properties.

Benefits of technology

It significantly improves the thermal insulation and flame retardant properties of the coating, prevents aluminum powder oxidation, enhances the stability and corrosion resistance of the coating, effectively reduces heat transfer and fire spread, and improves the overall safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027175130000081
    Figure BDA0005027175130000081
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, and particularly discloses a heat-insulating flame-retardant anticorrosive coating and a preparation method thereof. The invention relates to a heat-insulating flame-retardant anticorrosive coating, which is prepared from the following raw materials in parts by weight: 50 to 80 parts of silicone acrylic emulsion, 10 to 15 parts of epoxy resin, 30 to 40 parts of heat-insulating microcapsules, 15 to 21 parts of hollow glass beads, 3 to 5 parts of dispersing agents, 0.5 to 2 parts of polypropylene glycol diglycidyl ether, 1 to 5 parts of flatting agents and 15 to 20 parts of water, the capsule wall layer is made of acrylic resin and polyamide resin; the preparation method comprises the following steps: adding the hollow glass beads and the heat-insulating microcapsules into the silicone-acrylic emulsion and water, and uniformly dispersing to obtain a mixed solution; adding the dispersing agent, the polypropylene glycol diglycidyl ether, the epoxy resin and the flatting agent into the mixed solution, and uniformly mixing to obtain the interior wall thermal insulation coating. The composition provided by the invention realizes comprehensive improvement of heat insulation, flame retardance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of coatings, and more specifically, to a heat-insulating, flame-retardant and anti-corrosion coating and a preparation method thereof. Background Art

[0002] With the rapid development of modern industrial technology and the acceleration of urbanization, the operating environment faced by buildings, vehicles, power equipment and various industrial facilities is becoming increasingly complex and changeable, which puts higher requirements on the comprehensive performance of coatings, especially the heat insulation and flame retardant capabilities of anti-corrosion coatings have become the focus of attention.

[0003] Although traditional anti-corrosion coatings have played a certain role in preventing metal corrosion and extending the service life of equipment, their inadequacies in heat insulation and flame retardancy are gradually exposed when facing extreme environments such as high temperature and fire. Under high temperature conditions, the heat insulation effect of traditional anti-corrosion coatings is limited, and it is difficult to effectively prevent heat from being transferred to the substrate, causing the substrate temperature to rise sharply, which may cause safety accidents or accelerate material aging. At the same time, when a fire occurs, the flame retardant ability of traditional anti-corrosion coatings is insufficient and cannot effectively prevent the spread of the fire, increasing the risk of fire.

[0004] In order to improve the comprehensive performance of anti-corrosion coatings, especially their heat insulation and flame retardancy, it is urgent to develop a new type of coating. Summary of the invention

[0005] In order to improve the heat insulation and flame retardant capabilities of anti-corrosion coatings, the present application provides a heat insulation and flame retardant anti-corrosion coating and a preparation method thereof.

[0006] In the first aspect, the present application provides a heat-insulating, flame-retardant and anti-corrosion coating, which adopts the following technical solution: A heat-insulating, flame-retardant and anti-corrosion coating, comprising the following raw materials in parts by weight: 50-80 parts of silicone-acrylic emulsion, 10-15 parts of epoxy resin, 30-40 parts of thermal insulation microcapsules, 15-21 parts of hollow glass microspheres, 3-5 parts of dispersant, 0.5-2 parts of polypropylene glycol diglycidyl ether, 1-5 parts of leveling agent and 15-20 parts of water. The thermal insulation microcapsules include an aluminum powder core and a thermal insulation and flame retardant capsule wall layer, and the capsule wall layer material includes acrylic resin and polyamide resin.

[0007] By adopting the above technical scheme, the aluminum powder has metallic properties, not only has a high reflectivity for infrared rays, but also has a strong reflectivity for the entire wavelength band of sunlight, and the aluminum powder can be oriented and arranged in the coating to form a mirror surface during the drying and curing process of the coating, further improving the thermal insulation capacity of the coating. However, the aluminum powder is relatively active and easily reacts with oxygen, water, etc. in the air, which affects its performance. Therefore, acrylic resin and polyamide resin are used to encapsulate it to form thermal insulation microcapsules, which not only maintains the strong reflectivity of the aluminum powder for infrared rays and sunlight, significantly improves the thermal insulation performance of the coating, but also effectively prevents the oxidation of the aluminum powder, improves the stability and flame retardancy of the coating, and at the same time, the encapsulation of the aluminum powder improves the uniformity of the distribution of the aluminum powder in the base material, so that the aluminum powder can be more evenly dispersed in the base material to play its role.

[0008] In the process of preparing microcapsules, the electrons on the methyl α carbon atom in acrylic resin can react with the surface active aluminum, so that acrylic resin can adhere to the surface of aluminum powder to form a coating layer. The further addition of polyamide resin enhances the compatibility of acrylic resin and epoxy resin. A three-dimensional network structure is formed under the cross-linking action of polyamide, acrylic acid, silicone acrylic emulsion and epoxy resin, making the coating more dense and defect-free, reducing the penetration of combustible gas and oxygen, and further improving the flame retardant performance of the coating.

[0009] Epoxy primers with high anti-corrosion performance and strong adhesion are prepared using highly heat-resistant epoxy resins. Epoxy resins and silicone-acrylic emulsions are used as film-forming substances to synergistically construct a strong and anti-corrosion coating base. The addition of hollow glass microspheres further reduces the thermal conductivity of the coating and enhances the thermal insulation effect.

[0010] Optionally, the thermal insulation microcapsules are prepared by the following method: (1) After mixing aluminum powder and acetone for 20-30 minutes, ultrasonically disperse for 8-10 minutes, filter, wash, and set aside; (2) dissolving acrylic resin and polyamide resin in ethanol to form a capsule wall layer solution, adding the aluminum powder in step (1), stirring and mixing, and vacuum spray drying to obtain thermal insulation microcapsules; wherein the mass ratio of the acrylic resin to the polyamide resin is 1:2-3, and the mass ratio of the aluminum powder to the capsule wall layer solution is 1:1.2-1.5.

[0011] By adopting the above technical scheme, aluminum powder particles can be effectively dispersed in acetone to avoid agglomeration and agglomeration between aluminum powder particles, making it easier to proceed with subsequent processing steps. A silane coupling agent is further used to form a chemically bonded film on the surface of the silane coupling agent to improve the compatibility and bonding force between the aluminum powder and the capsule wall resin layers. The composite use of acrylic resin and polyamide resin forms capsule wall layers with low thermal conductivity, effectively reducing heat transfer and further improving the flame retardant and heat resistant properties of the coating.

[0012] Optionally, the rotation speed during the stirring process is 600-800 rpm.

[0013] By adopting the above technical solution, the surface tension of the coating increases when the coating solidifies and shrinks, and the two-dimensional aluminum powder in the polymer matrix tends to be oriented parallel to the substrate as the tension of the coating increases, thereby forming a planar structure parallel to the substrate in the coating, thereby having stronger reflective properties. Therefore, the basic form of the aluminum powder is crucial to the infrared reflective performance of the coating. By selecting a suitable stirring rate, the aluminum powder can be evenly dispersed while ensuring that the aluminum powder shape is not destroyed and is evenly spread in the coating, so that the prepared microcapsules have better thermal insulation effect.

[0014] Optionally, the particle size of the aluminum powder is between 10-60 μm.

[0015] By adopting the above technical solution, the particle size of the aluminum powder is further controlled to narrow the distribution range of the particle size, thereby achieving uniform distribution of the particle size and enhancing the flatness and consistency of the coating. The aluminum powder particles within this particle size range have a higher specific surface area, which enables more and denser reflective surfaces to be formed inside the coating, effectively improving the thermal insulation effect of the coating. At the same time, the aluminum powder particles within this particle size range are easier to achieve directional arrangement during the curing process of the coating. This orderly arrangement structure further enhances the thermal insulation effect of the coating, allowing the coating to reach a new height in thermal insulation performance.

[0016] Optionally, antimony-doped tin dioxide is further added to the inner core of the thermal insulation microcapsule, and the addition ratio of the aluminum powder to the antimony-doped tin dioxide is 1:0.2-0.4.

[0017] By adopting the above technical solution, antimony-doped tin dioxide has excellent thermal insulation properties, which, combined with the metallic luster and reflective properties of aluminum powder, can form a microcapsule structure with a dual thermal insulation mechanism. This structure not only enhances the coating's ability to reflect infrared and sunlight, but also further blocks the heat transfer path through the antimony-doped tin dioxide's own thermal insulation properties. In addition, the low thermal expansion coefficient of antimony-doped tin dioxide plays a key role when the coating is heated, helping to maintain the stability of the coating, reducing cracks and peeling caused by thermal expansion differences, and further enhancing the overall flame retardant effect of the coating.

[0018] Optionally, the dispersant is any one of fatty alcohol polyoxyethylene ether and polycarboxylate dispersants.

[0019] By adopting the above technical solution, the various components of the raw materials can be evenly dispersed to obtain an anti-corrosion coating with good heat insulation effect and flame retardancy.

[0020] Optionally, 2-3 parts of potassium methyl silicate are also added to the raw materials.

[0021] By adopting the above technical solution, potassium methyl silicate can react with silicone acrylic emulsion to form a dense protective film on the surface of the coating, which can isolate the contact between the corrosive medium and the coating substrate and improve the corrosion resistance of the coating. At the same time, when the surface of the coating is burned by flames, this protective film can serve as a heat insulation barrier to slow down the transfer of flames and heat to the inside of the coating, effectively improving the flame retardant properties of the coating.

[0022] In a second aspect, the present application provides a method for preparing a heat-insulating, flame-retardant, and anti-corrosion coating, which adopts the following technical scheme: A method for preparing a heat-insulating, flame-retardant, and anti-corrosion coating, comprising the following preparation steps: (1) adding hollow glass microspheres and heat-insulating microcapsules into silicone-acrylic emulsion and water and dispersing them uniformly to obtain a mixed solution; (2) Add a dispersant, polypropylene glycol diglycidyl ether, epoxy resin and a leveling agent to the mixed solution and mix them evenly to obtain the interior wall thermal insulation coating.

[0023] By adopting the above technical scheme, the preparation process is simple, the dispersibility of the filler in the coating is improved, and the components can be fully mixed to obtain an anti-corrosion coating with excellent heat insulation and flame retardant properties.

[0024] In summary, this application has the following beneficial effects: 1. Since the present application introduces heat-insulating microcapsules, the aluminum powder core has strong reflective ability to infrared and sunlight, effectively reducing the absorption of heat. At the same time, the capsule wall layer of the heat-insulating capsule is made of acrylic resin and polyamide resin, which has a low thermal conductivity, further blocking the heat transfer path, while protecting the aluminum powder from being easily oxidized and ineffective. The addition of hollow glass microspheres further reduces the thermal conductivity of the coating and enhances the overall thermal insulation effect. The multiple thermal insulation mechanisms make the coating have higher thermal insulation performance.

[0025] 2. The epoxy resin and silicone-acrylic emulsion in the coating of this application work together to construct a strong and corrosion-resistant coating base, which improves the adhesion and corrosion resistance of the coating. The addition of potassium methyl silicate forms a dense protective film on the surface of the coating, which effectively isolates the contact between the corrosive medium and the substrate, further enhancing the corrosion resistance of the coating. At the same time, the protective film can also serve as a heat insulation barrier, slowing down the transfer of heat to the interior of the coating at high temperatures and improving the flame retardant properties of the coating. In addition, the antimony-doped tin dioxide in the insulating microcapsules not only enhances the thermal insulation effect of the coating, but also helps to maintain the stability of the coating due to its low thermal expansion coefficient characteristics, reducing cracks and peeling caused by thermal expansion differences, thereby further enhancing the overall flame retardant effect of the coating. DETAILED DESCRIPTION

[0026] The present application is further described in detail below with reference to the embodiments.

[0027] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0028] Polyamide resin was purchased from Dongguan Jincan Plastic New Materials Co., Ltd., brand 8202C; epoxy resin was purchased from Langfang Nanze Anticorrosion Materials Co., Ltd., brand: E-44; aluminum powder was purchased from Xinji Guangyuan Metal Powder Leaf Co., Ltd.; antimony-doped tin dioxide was purchased from Hangzhou Jiupeng New Materials Co., Ltd., model: CY-G06, particle size 30 nm.

[0029] Preparation examples of raw materials and / or intermediates Preparation Example 1 A heat-insulating microcapsule, the preparation of which comprises the following steps: (1) 50 kg of aluminum powder and acetone were stirred and mixed at a rate of 600 rpm for 20 min, and then ultrasonically dispersed for 10 min, filtered, washed with clean water, and set aside. The amount of acetone used was based on the amount that could immerse the aluminum powder; (2) dissolving acrylic resin and polyamide resin in twice the amount of ethanol solution to form a capsule wall layer solution, adding the aluminum powder in step (1) and stirring at a rate of 600 rpm to mix, and then vacuum spray drying at an inlet air temperature of 40° C., an outlet air temperature of 30° C., and a vacuum degree of -0.09 MPa to obtain thermal insulation microcapsules; wherein the mass ratio of the acrylic resin to the polyamide resin is 1:2.5, and the mass ratio of the aluminum powder to the capsule wall layer solution is 1:1.35; and the particle size of the aluminum powder is between 10 and 60 μm.

[0030] Preparation Example 2 A heat-insulating microcapsule, the preparation of which comprises the following steps: (1) 50 kg of aluminum powder and acetone were stirred and mixed at a rate of 800 rpm for 8 minutes, and then ultrasonically dispersed for 5 minutes, filtered, washed with clean water, and set aside. The amount of acetone used was based on the amount that could immerse the aluminum powder; (2) dissolving acrylic resin and polyamide resin in twice the amount of ethanol solution to form a capsule wall layer solution, adding the aluminum powder in step (1) and stirring at a rate of 800 rpm to mix, and then vacuum spray drying at an inlet air temperature of 40° C., an outlet air temperature of 30° C., and a vacuum degree of -0.09 MPa to obtain thermal insulation microcapsules; wherein the mass ratio of the acrylic resin to the polyamide resin is 1:3, and the mass ratio of the aluminum powder to the capsule wall layer solution is 1:1.2; and the particle size of the aluminum powder is between 10 and 60 μm.

[0031] Preparation Example 3 A heat-insulating microcapsule, the preparation of which comprises the following steps: (1) 50 kg of aluminum powder and acetone were stirred and mixed at a rate of 700 rpm for 25 min, and then ultrasonically dispersed for 9 min, filtered, washed with clean water, and set aside. The amount of acetone used was based on the amount that could immerse the aluminum powder; (2) dissolving acrylic resin and polyamide resin in twice the amount of ethanol solution to form a capsule wall layer solution, adding the aluminum powder in step (1) and stirring at a rate of 700 rpm to mix, and then vacuum spray drying at an inlet air temperature of 40° C., an outlet air temperature of 30° C., and a vacuum degree of -0.09 MPa to obtain thermal insulating microcapsules; wherein the mass ratio of the acrylic resin to the polyamide resin is 1:2, and the mass ratio of the aluminum powder to the capsule wall layer solution is 1:1.5; and the particle size of the aluminum powder is between 10 and 60 μm.

[0032] Preparation Example 4 A heat-insulating microcapsule, which is different from Preparation Example 1 in that the stirring mixing speed of 900 rpm is used for 20 minutes in this Preparation Example.

[0033] Preparation Example 5 A heat-insulating microcapsule, which is different from Preparation Example 1 in that in this Preparation Example, when treating aluminum powder, a stirring mixing rate of 500 rpm is used for 20 minutes.

[0034] Preparation Example 6 A heat-insulating microcapsule, which is different from Preparation Example 1 in that the aluminum powder used in this Preparation Example has a particle size of 20-100 μm.

[0035] Preparation Example 7 A heat-insulating microcapsule, which is different from Preparation Example 1 in that antimony-doped tin dioxide is also added in this Preparation Example, and the preparation comprises the following steps: (1) 50 kg of aluminum powder and acetone were stirred and mixed at a rate of 600 rpm for 20 min, and then ultrasonically dispersed for 10 min, filtered, washed with clean water, and set aside. The amount of acetone used was based on the amount that could immerse the aluminum powder; (2) dissolving acrylic resin and polyamide resin in two times the mass of ethanol solution to form a capsule wall layer solution, adding 10 kg of antimony-doped tin dioxide and the aluminum powder in step (1) and stirring at a rate of 600 rpm to mix, and then vacuum spray drying at an inlet air temperature of 40° C., an outlet air temperature of 30° C., and a vacuum degree of -0.09 MPa to obtain thermal insulation microcapsules; wherein the added mass ratio of acrylic resin to polyamide resin is 1:2.5, and the added mass ratio of aluminum powder to capsule wall layer solution is 1:1.35; and the particle size of the aluminum powder is between 10 and 60 μm.

[0036] Preparation Example 8 A heat-insulating microcapsule, which is different from Preparation Example 7 in that the ratio of aluminum powder to antimony-doped tin dioxide in this Preparation Example is 1:0.4.

[0037] Comparative Preparation Example 1 A heat-insulating microcapsule, which is different from Preparation Example 1 in that the capsule wall material in this Preparation Example is replaced by an equal amount of acrylic resin instead of polyamide resin.

[0038] Comparative Preparation Example 2 A heat-insulating microcapsule, which is different from Preparation Example 1 in that the capsule wall material in this Preparation Example is replaced by an equal amount of polyamide resin instead of acrylic resin. Example

[0039] Example 1 A heat-insulating, flame-retardant and anti-corrosion coating, the preparation of which comprises the following steps: (1) adding 18 kg of hollow glass microspheres and 35 kg of thermal insulation microcapsules to 65 kg of silicone-acrylic emulsion and 20 kg of water and dispersing them uniformly to obtain a mixed solution; (2) Add 4 kg of fatty alcohol polyoxyethylene ether (dispersant), 1 kg of polypropylene glycol diglycidyl ether, 15 kg of epoxy resin and 2.5 kg of leveling agent 5400 to the above mixed liquid and mix evenly to obtain the interior wall insulation coating; in this embodiment, the thermal insulation microcapsules prepared in Preparation Example 1 are used.

[0040] Example 2 A heat-insulating, flame-retardant and anti-corrosion coating, the preparation of which comprises the following steps: (1) adding 21 kg of hollow glass microspheres and 30 kg of thermal insulation microcapsules to 80 kg of silicone-acrylic emulsion and 20 kg of water and dispersing them evenly to obtain a mixed solution; (2) Add 3 kg of fatty alcohol polyoxyethylene ether (dispersant), 2 kg of polypropylene glycol diglycidyl ether, 12.5 kg of epoxy resin and 5 kg of leveling agent 5400 to the above mixed liquid and mix evenly to obtain the interior wall insulation coating; in this embodiment, the thermal insulation microcapsules prepared in Preparation Example 2 are used.

[0041] Example 3 (1) adding 15 kg of hollow glass microspheres and 40 kg of thermal insulation microcapsules to 50 kg of silicone-acrylic emulsion and 20 kg of water and dispersing them evenly to obtain a mixed solution; (2) Add 5 kg of fatty alcohol polyoxyethylene ether (dispersant), 0.5 kg of polypropylene glycol diglycidyl ether, 10 kg of epoxy resin and 1 kg of leveling agent 5400 to the above mixed solution and mix evenly to obtain the interior wall insulation coating; in this embodiment, the thermal insulation microcapsules prepared in Preparation Example 3 are used.

[0042] Embodiment 4-8 A heat-insulating, flame-retardant and anti-corrosion coating is prepared according to the method in Example 1, except that the heat-insulating microcapsules added therein are those prepared in Preparation Examples 4-8.

[0043] Example 9 A heat-insulating, flame-retardant and anti-corrosion coating, which is different from Example 1 in that 2 kg of potassium methyl silicate is added in this embodiment, and the preparation comprises the following steps: (1) adding 18 kg of hollow glass microspheres and 35 kg of thermal insulation microcapsules to 65 kg of silicone-acrylic emulsion and 20 kg of water and dispersing them uniformly to obtain a mixed solution; (2) 4 kg of fatty alcohol polyoxyethylene ether (dispersant), 1 kg of polypropylene glycol diglycidyl ether, 15 kg of epoxy resin, 2 kg of potassium methyl silicate and 2.5 kg of leveling agent 5400 were added to the above mixed solution and mixed evenly to obtain the interior wall insulation coating; in this embodiment, the thermal insulation microcapsules prepared in Preparation Example 1 were used.

[0044] Example 10 A heat-insulating, flame-retardant and anti-corrosion coating, which is different from Example 9 in that 3 kg of potassium methyl silicate is added in this example.

[0045] Comparative Example Comparative Example 1 A heat-insulating, flame-retardant and anti-corrosion coating, which is different from Example 1 in that an equal amount of aluminum powder is used in this comparative example instead of heat-insulating microcapsules.

[0046] Comparative Example 2 A heat-insulating, flame-retardant and anti-corrosion coating, which is different from Example 1 in that the heat-insulating microcapsules added in this comparative example are prepared in Comparative Preparation Example 1.

[0047] Comparative Example 3 A heat-insulating, flame-retardant and anti-corrosion coating, which is different from Example 1 in that the heat-insulating microcapsules added in this comparative example are prepared in Comparative Preparation Example 2.

[0048] Performance testing Detection method / test method Solar reflection and heat insulation performance test: According to the standard JC / T 1040-2020 "Heat-reflective and heat-insulating coatings for exterior surfaces of buildings", the solar reflectivity of the coating is tested. The higher the reflectivity, the better the heat insulation capacity; Flame retardant performance: oxygen index is tested in accordance with GB / T 8624-2012 "Classification of Combustion Performance of Building Materials and Products"; Thermal conductivity: The thermal conductivity of the coating is obtained by testing according to the ASTM E1530 coating thermal conductivity test standard; Heat resistance: Use a spray gun to spray the coating on a Q235 steel plate to prepare a coating sample with a thickness of 50 μm. After complete curing, place it in the air for curing for 48 hours, and then test its impact resistance according to GB / T 1732-2020 "Determination of impact resistance of paint film". Then, place it in an electric constant temperature blower for heat treatment at 120°C. After 3 days, take it out and cool it to room temperature, and test its impact strength again. The data are recorded in Table 1. At the same time, observe whether the coating has any coating failure phenomena such as rust, bubbles, shedding, powdering, cracking or discoloration.

[0049] Table 1 Test results Combining Examples 1-3 and Comparative Example 1 and Table 1, it can be seen that the test data of Examples 1-3 are better than those of Comparative Example 1, indicating that the preparation of thermal insulation microcapsules can improve the thermal insulation and flame retardant properties of the coating, effectively prevent the oxidation of aluminum powder particles, and improve the stability of the coating performance.

[0050] Combining Examples 1-3 and Comparative Examples 2-3 and Table 1, it can be seen that the experimental data of Examples 1-3 are better than those of Comparative Examples 2-3, indicating that the wrapping layer formed by acrylic resin and polyamide resin has better heat insulation ability and improves the flame retardant ability of the coating.

[0051] It can be seen from Examples 1-5 and Table 1 that the experimental data of Examples 1-3 are better than those of Examples 4-5, indicating that the stirring rate in the process of preparing microcapsules affects the morphology of aluminum powder. The stirring rate is controlled between 600-800 rpm so that the aluminum powder can be evenly dispersed while maintaining its morphology, so that it can be better spread in the coating, exert its reflective properties, and improve the thermal insulation ability of the coating.

[0052] Combining Example 1 with Example 6 and Table 1, it can be seen that the experimental data of Example 1 are better than those of Example 6, indicating that when the particle size range of the aluminum powder is large, the particle size distribution is combined with Example 1 with Examples 7-8 and Table 1, it can be seen that the experimental data of Examples 7-8 are better than those of Example 1, indicating that adding a small amount of antimony-doped tin dioxide is beneficial to the cooperation with aluminum powder, which not only enhances the coating's ability to reflect heat, but also utilizes its good thermal insulation properties to further block the heat transfer path and improve the thermal insulation and flame retardant capabilities of the coating.

[0053] Combining Example 1 with Examples 9-10 and Table 1, it can be seen that the test data of Examples 9-10 are better than those of Example 1, indicating that the addition of potassium methyl silicate is beneficial to forming a dense protective film on the surface of the coating, preventing heat from being transferred to the inside of the coating, thereby improving the flame retardant properties of the coating.

[0054] The coating was placed in an electric constant temperature blower at 120°C for a long time, taken out and cooled to room temperature after 3d, 7d, 14d and 28d respectively, and its surface was observed. It was recorded that the coatings prepared in the examples of the present application did not show any coating failure phenomena such as rust, bubbles, shedding, powdering, cracking or discoloration, indicating that the coatings prepared by the method of the present application have good high temperature resistance and can still maintain good performance in a long-term high temperature environment.

[0055] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A heat-insulating, flame-retardant and anti-corrosion coating, characterized in that: The composition comprises the following raw materials in parts by weight: 50-80 parts of silicone-acrylic emulsion, 10-15 parts of epoxy resin, 30-40 parts of thermal insulation microcapsules, 15-21 parts of hollow glass microspheres, 3-5 parts of dispersant, 0.5-2 parts of polypropylene glycol diglycidyl ether, 1-5 parts of leveling agent and 15-20 parts of water. The thermal insulation microcapsules include an aluminum powder core and a thermal insulation and flame retardant capsule wall layer, and the capsule wall layer material includes acrylic resin and polyamide resin.

2. The heat-insulating, flame-retardant and anti-corrosion coating according to claim 1, characterized in that: The thermal insulation microcapsules are prepared by the following method: (1) Stir and mix aluminum powder and acetone for 20-30 minutes, then ultrasonically disperse for 8-10 minutes, filter, wash and set aside; (2) dissolving acrylic resin and polyamide resin in ethanol to form a capsule wall layer solution, adding the aluminum powder in step (1), stirring and mixing, and vacuum spray drying to obtain thermal insulation microcapsules; wherein the mass ratio of the acrylic resin to the polyamide resin is 1:2-3, and the mass ratio of the aluminum powder to the capsule wall layer solution is 1:1.2-1.

5.

3. The heat-insulating, flame-retardant and anti-corrosion coating according to claim 2, characterized in that: The rotation speed during the stirring process is 600-800 rpm.

4. The heat-insulating, flame-retardant and anti-corrosion coating according to claim 1, characterized in that: The particle size of the aluminum powder is between 10-60 μm.

5. The heat-insulating, flame-retardant and anti-corrosion coating according to claim 1, characterized in that: Antimony-doped tin dioxide is also added to the inner core of the heat-insulating microcapsule, and the addition ratio of the aluminum powder to the antimony-doped tin dioxide is 1:0.2-0.

4.

6. The heat-insulating, flame-retardant and anti-corrosion coating according to claim 1, characterized in that: The dispersant is any one of fatty alcohol polyoxyethylene ether and polycarboxylate dispersants.

7. The heat-insulating, flame-retardant and anti-corrosion coating according to claim 1, characterized in that: 2-3 parts of potassium methyl silicate are also added to the raw materials.

8. A method for preparing a heat-insulating, flame-retardant, and anti-corrosion coating according to any one of claims 1 to 7, characterized in that: The method comprises the following preparation steps: (1) adding hollow glass microspheres and thermal insulation microcapsules into silicone-acrylic emulsion and water and dispersing them evenly to obtain a mixed solution; (2) Add a dispersant, polypropylene glycol diglycidyl ether, epoxy resin and a leveling agent to the mixed liquid and mix them evenly to obtain the interior wall thermal insulation coating.

Citation Information

Patent Citations

  • Acrylic heat insulation coating with high reflectivity and preparation method of acrylic heat insulating coating

    CN109233493A

  • Coated aluminum powder and preparation method thereof, and silver-white aluminum powder paint and preparation method thereof

    CN113025081A

  • Flame-retardant microcapsule curd, water-based flame-retardant anticorrosive plastic coating and preparation method thereof

    CN114196267A

  • A heat storage material in microcapsule form having organic and inorganic bilayer coat, and a preparation method thereof

    KR100715455B1

  • Aluminum powder used for 3D printing, and method for preparation of said aluminum powder

    WO2016119556A1

Cited By

  • Multifunctional fireproof anticorrosive paint and production process thereof

    CN119552549A