Fireproof coating

By combining modified urea formaldehyde resin and VAE emulsion, combined with expandable vermiculite and other fillers, the problem that existing fire-retardant coatings are difficult to have both fire-retardant and waterproof performance, achieving application needs in the high-end market, and cost control is effective.

CN118931304AActive Publication Date: 2024-11-12BEIJING GANGAN TECH CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411177932.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing expansion fire-retardant coatings are difficult to have excellent fire-retardant and water-retardant properties at the same time, resulting in limited applications in the high-end fire-retardant market.

Method used

Modified urea formaldehyde resin and vinyl acetate-ethylene copolymer (VAE) emulsion as the main film forming substances, combined with expandable vermiculite, low-molecular carbon source, carbon-forming catalyst and foaming agent, through alkali-acid-base process Prepare modified urea formaldehyde resin and add titanium dioxide and other fillers to improve the waterproofness and fire resistance of the paint.

Benefits of technology

It achieves excellent fire resistance and waterproof performance of coatings, is suitable for the high-end fireproof market, and the cost is controlled within an acceptable range.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a fireproof coating, which is characterized by comprising the following components in percentage by weight: 10 to 30 percent of vinyl acetate-ethylene copolymer (VAE) emulsion, 10 to 30 percent of modified urea resin, 5 to 20 percent of expansible vermiculite, 10 to 30 percent of coating additive and other filler, 10 to 30 percent of intumescent flame retardant and 5 to 30 percent of water, wherein the modified urea-formaldehyde resin is obtained by carrying out chemical coating modification on melamine modified urea-formaldehyde resin by utilizing polyacrylate. The fireproof coating is good in expansion performance, excellent in fireproof performance and good in waterproofness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fireproof coating. Furthermore, the fireproof coating contains a modified urea-formaldehyde resin specially used for fireproof materials. The modified urea-formaldehyde resin is obtained by chemically coating and modifying melamine-modified urea-formaldehyde resin with polyacrylate. Background Art

[0002] Expandable fire retardant coatings are mainly used for fire protection of steel structures. Economic and social development has promoted the development of the construction industry. Large buildings such as exhibition halls, terminal buildings, large shopping malls, stadiums, high-end hotels and industrial plants are increasing, and are developing in the direction of large size and beauty. Their main load-bearing components are mostly steel structures.

[0003] For this reason, fire prevention of steel structures has attracted more and more attention. Although steel is a non-combustible material, its fire resistance is far worse than that of masonry and reinforced concrete structures. As the temperature rises, the mechanical strength of steel will decrease. When the temperature rises to the critical temperature of steel (generally 540°C), its yield stress is only 40% of that at room temperature. Steel has a fire resistance limit of only 15 minutes under direct burning of high-temperature flames. The use of fire retardant coatings is an ideal method for fire prevention of steel structures. Steel structure fire retardant coatings are applied to the surface of steel components to play a role in fireproofing and heat insulation protection, preventing steel from rapidly heating up and reducing strength in a fire, and avoiding the collapse of the building due to the loss of support of the steel structure.

[0004] Steel structure fire retardant coatings can generally be divided into thick coating type, thin coating type and ultra-thin type. From the development trend, ultra-thin steel structure fire retardant coatings will eventually replace thick coating type and thin coating type fire retardant materials. Thin or ultra-thin fire retardant coatings are a kind of fire retardant coatings made of water-based resin as film-forming material and compounded with intumescent flame retardants that can form a coating with the film-forming material. This kind of coating is both decorative and fireproof. When exposed to fire, the coating can expand to more than dozens of times its original thickness, forming a porous carbonized layer to protect the substrate from burning and has a heat insulation effect.

[0005] General intumescent flame retardants are usually mixed with catalysts composed of phosphorus-containing substances (phosphorus sources), carbon-forming agents composed of polyhydroxy organic substances (carbon sources), and foaming agents composed of nitrogen-containing organic substances (nitrogen sources), and are added to resins in large quantities. Amino resins (urea-formaldehyde resins, melamine formaldehyde resins, melamine urea-formaldehyde resins) contain rich carbon and nitrogen sources, and are both carbon-forming agents and foaming agents, which can reduce the amount of added flame retardants. Fire-retardant coatings prepared with amino resins as film-forming materials have good foaming properties.

[0006] The amino resin itself is a multi-functional structure. The cross-linking density of the coating after room temperature curing is large. The coating is hard and brittle, and the flexibility is poor. The cured coating is prone to cracking after being placed for a short time. In order to solve the above technical problems, CN114250023A discloses a fire retardant coating and a preparation method. The mass fractions of the components taken are: 60% to 70% of water-based amino resin, 20% to 30% of expansion flame retardant and 5% to 10% of self-repairing microcapsules; a film-forming aid corresponding to the capsule core of the self-repairing microcapsule is also added; the water-based amino resin is selected from one or more combinations of urea-formaldehyde resin, melamine formaldehyde resin, and melamine urea-formaldehyde resin; the expansion flame retardant is a mixed or reactive expansion flame retardant; the wall material of the self-repairing microcapsule is melamine urea-formaldehyde resin or urea-formaldehyde resin, and the capsule core is a water-based room temperature self-crosslinking resin. However, the preparation process of this coating is relatively complicated and has poor waterproofness.

[0007] Prior art CN114213912A discloses a multifunctional water-based paint and a preparation method thereof. Wherein, taking the total mass of the multifunctional water-based paint as 100%, the multifunctional water-based paint includes the following raw material components: 10-30% of vinyl acetate-ethylene copolymer emulsion, 10-30% of elastic emulsion, 2-5% of anti-rust pigment, 1-2% of anti-flash rust agent, 0.3-1% of mildew and preservative, 0.5-1.5% of silane coupling agent, 30-40% of flame retardant pigment and filler, 1-10% of auxiliary additive, and the balance of water. The multifunctional water-based paint provided in this application enables the water-based paint to have fireproofing, waterproofing and anti-corrosion properties at the same time. The applicant used the patent formula and found that in order to overcome the problem of weak waterproofness of the vinyl acetate-ethylene copolymer film-forming material, a large amount of elastic emulsion was added to the formula. Although elastic emulsions can improve waterproof performance, their role in promoting foam formation and maintaining foam stability and integrity is much inferior to that of VAE emulsions and urea-formaldehyde resins, which means that the fire resistance of the coating is reduced. Therefore, the formula needs to add up to 30-40% of flame retardant pigments and fillers composed of pentaerythritol, melamine, ammonium polyphosphate and titanium dioxide to ensure fire resistance. This greatly increases the cost of the coating and is not suitable for the current highly competitive coating market.

[0008] And general urea-formaldehyde resin, especially melamine-modified urea-formaldehyde resin (MUF), is widely used in wood manufacturing industry, for bonding wood or being applied to wood-based material production as adhesive, for example, in the production of particleboard, plywood and various fiberboards.Urea-formaldehyde resin is the reaction product of urea and formaldehyde.Due to the poor water resistance and strength of this urea-formaldehyde resin, urea-formaldehyde resin modifier is generally used to modify the urea-formaldehyde resin obtained, to obtain modified urea-formaldehyde resin such as commonly used melamine-modified urea-formaldehyde resin (MUF), the water resistance and strength of this urea-formaldehyde resin are significantly higher than unmodified conventional urea-formaldehyde resin.Described urea-formaldehyde resin modifier is generally melamine, phenol or resorcinol, acrylate copolymer solution, isocyanate, polyvinyl alcohol, lignin etc. For example, CN102898604A discloses a method for preparing a modified urea-formaldehyde resin with improved storage stability, which comprises: (1) subjecting the first batch of urea, a modifier and formaldehyde to a first contact reaction until the water miscibility is 0.4 to 1.5 times, and the molar ratio of formaldehyde to the total amount of the first batch of urea and the modifier is 1 to 1.7:1; (2) subjecting the obtained mixture to a second contact reaction with the second batch of urea at a temperature of 60±15°C for 1 to 30 minutes, and the molar ratio of formaldehyde to the total amount of the first batch of urea, the second batch of urea and the modifier is 0.6 to 1.25:1; (3) adjusting the pH value of the mixture obtained in step (2) to 8.5 to 10 and cooling to below 40°C. The modifier is at least one of melamine, phenol, resorcinol, isocyanate, polyvinyl alcohol and lignin. The above-mentioned urea-formaldehyde resin is mainly for improving storage stability and reducing formaldehyde release. The water resistance of the modified urea-formaldehyde resin is improved, but it is still not comparable to the water resistance of acrylic resin and cannot meet the water resistance requirements of fire retardant coatings.

[0009] In short, after actual market research, it is found that thin fire-retardant coatings currently mainly use vinyl acetate-ethylene copolymers, polyacrylate polymers, etc. as film-forming materials, while urea-formaldehyde resin can be used as both a carbon source and a nitrogen source, and is both a carbon former and a foaming agent. It is generally used as an auxiliary resin. This is because even the modified phenolic resin is not as waterproof as the acrylic resin, and its fireproof performance is slightly inferior to the Wacker 3066 emulsion used in the mainstream high-end fireproof material market. Compared with the fireproof performance of Wacker 3066 emulsion, it can only be used as an auxiliary film-forming material, and the addition amount cannot be too high. Even if melamine and or isocyanate-modified urea-formaldehyde resin is used, although it can increase the stability and other properties of fire-retardant coatings, the waterproofness still cannot meet the requirements of the high-end fireproof market. Even if the elastic emulsion with better waterproofness is used for modification, the waterproofness has improved, but the improvement of physical blending modification is limited. In addition, if the amount of elastic emulsion is too much, it will inhibit the generation of foam, thereby affecting the fireproof performance. It can be seen that the current urea-formaldehyde resins on the market are difficult to balance fire resistance and water resistance. Although polyacrylate elastic emulsions have good water resistance, they are not fire resistant. VAE emulsions represented by Wacker 3066 emulsions have excellent fire resistance, but poor water resistance. Even if the two are blended, the water resistance and fire resistance are reduced. In other words, the current intumescent fire retardant coatings that use vinyl acetate-ethylene copolymers, polyacrylate polymers and urea-formaldehyde resins as film-forming materials are difficult to have excellent fire resistance and water resistance at the same time. Summary of the invention

[0010] The purpose of the present application is to provide a fire retardant coating, which has both excellent fire retardant and waterproof properties, characterized in that it comprises the following components in weight percentage: 10-30% of vinyl acetate-ethylene copolymer (VAE) emulsion, 10-30% of modified urea-formaldehyde resin, 5-20% of expandable vermiculite, 10-30% of coating additives and other fillers, 10-30% of intumescent flame retardant, and 5-30% of water; The intumescent flame retardant is composed of a low molecular carbon source, a carbon-forming catalyst and a foaming agent, the low molecular carbon source is pentaerythritol, dipentaerythritol or tripentaerythritol, the carbon-forming catalyst is ammonium polyphosphate, diammonium phosphate, monoammonium phosphate, ammonium metaphosphate, ammonium hypophosphite, ammonium phosphite, phosphorous acid, metaphosphoric acid and / or orthophosphoric acid, and the foaming agent is melamine, dicyandiamide, ammonium oxalate, urea or hexamethylenetetramine; wherein, in terms of mass ratio, the weight ratio of the low molecular carbon source, the carbon-forming catalyst and the foaming agent is (1-2):(1-2):(0.5-1.5); Preferably, the coating additives include defoamers, leveling agents, dispersants, thickeners and / or wetting agents. Preferably, the other filler includes titanium dioxide.

[0011] Preferably, other fillers include titanium dioxide, lithopone or heavy calcium carbonate.

[0012] The vinyl acetate-ethylene copolymer emulsion is selected from at least one of Wacker EZ 3066 and Wacker EZ 3112; The present application also discloses a manufacturing process of the modified urea-formaldehyde resin, which is manufactured by an alkali-acid-alkali process and comprises the following steps: (1) Add a certain mass of formaldehyde solution into the reactor, add a certain amount of deionized water, then adjust the pH to 7.5-9.0 with sodium hydroxide aqueous solution, and heat to 40-55°C, then add the first batch of urea and the first batch of melamine under stirring conditions, heat to 85-95°C and keep the temperature for 20-40 minutes or heat to 70-75°C and keep the temperature for 50-80 minutes; (2) Adjust the pH to 5.0-5.5 with formic acid, raise the temperature to 80-95°C, continue to keep the temperature for a period of time, and finally cool the reactants to 65-75°C, adjust the pH to 7.0-7.5 with sodium hydroxide aqueous solution, add the second batch of urea and the second batch of melamine, stir evenly, and keep the temperature for 20-40 minutes; (3) After cooling to a certain temperature, add the third batch of urea, keep the temperature at 70-90°C for 10-40 minutes, and then adjust the pH value to 8.0-9.0 to obtain a basic modified urea-formaldehyde resin; (4) Adding the pre-prepared mixture of isocyanate acrylate, acrylate and ester solvent while stirring, and reacting for 15-25 minutes; wherein the sum of the amounts of isocyanate acrylate and acrylate is 5-10 wt % based on the basic modified urea-formaldehyde resin.

[0013] (5) adding 5-10 wt% of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and acrylate mixture based on the basic modified urea-formaldehyde resin while stirring, the mass ratio of the two being (2-4):1; (6) Add initiator solution, raise the temperature to 50-90°C, and react for 0.4-3.5 hours to obtain modified urea-formaldehyde resin.

[0014] In steps (1) to (3), the cumulative molar ratio of formaldehyde to (urea + melamine) is 1.05-1.15; In step (2), the reaction is continued at a temperature of 16 to 20 seconds (Tu-4 cup, 30°C test) and then the reactants are cooled to 65 to 75°C. The weight ratio of isocyanate acrylate to acrylate in step (4) is (3-5): 1 In step (4), the isocyanate acrylate may be ethyl isocyanate acrylate or ethyl isocyanate methacrylate; The ester solvent in step (4) includes one or more of ethyl acetate, octyl acetate, and n-butyl acetate.

[0015] In step (4), the acrylate may be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate; In step (5), the acrylate may be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate; In step (6), the initiator is one or more of sodium persulfate, azobisisobutyronitrile, dibenzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, diisopropylbenzene peroxide, and di-tert-amyl peroxide; In summary, this application has the following beneficial effects: (1) This application uses titanium dioxide as a filler for fire-retardant coatings, which not only plays a common coloring role, but also plays a role in catalyzing foaming to improve fire-retardant performance. While using isocyanate to modify urea-formaldehyde resin, it also acts as a functional linker to achieve chemical grafting and coating modification of urea-formaldehyde resin by polyacrylate, thereby improving waterproof performance.

[0016] (2) Among many types of acrylic ester monomers, tri(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) was finally selected after a large number of experiments. While achieving the waterproofing effect of acrylic polymer coating, it also has the effect of foaming into carbon. It is speculated that this may be due to its nitrogen-containing characteristics, which avoids the acrylic resin with too low nitrogen content outside the urea-formaldehyde resin from inhibiting foaming into carbon.

[0017] (3) In step (4), the mixture is prepared by using a mixture of isocyanate acrylate, acrylate and ester solvents. On the one hand, the slow side reaction of isocyanate acrylate with water is reduced. On the other hand, by dispersing the isocyanate acrylate in the acrylate and ester solvents, local high cross-linking between the isocyanate acrylate and the urea-formaldehyde resin is avoided, which is conducive to the uniform coating of the isocyanate acrylate. Finally, the acrylate added together as a dispersion medium also increases the reaction response speed of the subsequent free radical copolymerization of the acrylate and the acrylic functional group in the isocyanate.

[0018] (4) The outer coating uses a mixture of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and acrylates to avoid the high cross-linking of THEICTA due to its three functional groups, which will increase the decomposition temperature and thus mismatch the decomposition and dehydration temperature of the intumescent flame retardant in the fireproof material, and even inhibit the early dehydration and foaming. Some acrylates can significantly reduce the cross-linking density, and while improving the bonding performance of the film-forming material, the effect of improving the foaming performance can be maintained.

[0019] (5) The amount of isocyanate acrylate should be appropriate. If it is too little, the coating effect is poor, and the effect of improving the waterproof effect and fire resistance is insufficient. If it is too much, isocyanate will consume a large amount of amino groups and even hydroxyl groups inside the urea-formaldehyde resin, and the hydroxyl content determines the dehydration and foaming rate of the urea-formaldehyde resin. Therefore, the amount of isocyanate acrylate should be appropriate. Example

[0020] Example 1 Preparation of modified urea-formaldehyde resin A The modified urea-formaldehyde resin is produced by an alkali-acid-alkali process, which includes the following steps: (1) Add a certain mass of 4.05 kg (48.6 moles) of formaldehyde solution (36%) into the reactor, add a certain amount of deionized water, then adjust the pH to 8.0 with 30% sodium hydroxide aqueous solution, and heat to 50°C. Then, add the first batch of urea 0.8 kg and the first batch of melamine 0.315 kg under stirring conditions, raise the temperature to 95°C and keep the temperature for 30 minutes; (2) Adjust the pH to 5.0 with 10 wt% formic acid, raise the temperature to 95°C, and continue to keep the temperature to react until the system viscosity reaches 18s (apply 4 cups, test at 30°C). Finally, cool the reactants to 70°C, adjust the pH to 7.0 with sodium hydroxide aqueous solution, add 1.0 kg of the second batch of urea and 0.315 kg of the second batch of melamine, stir evenly, and keep the temperature to react for 30 minutes; (3) After cooling to a certain temperature, add 0.6 kg of the third batch of urea, keep the temperature at 70°C for 20 minutes, cool to 40°C, and then adjust the pH value to 8.0 to obtain a basic modified urea-formaldehyde resin; (4) Add 0.354 kg of a mixture of ethyl isocyanate acrylate and ethyl acrylate (5 wt % based on urea-formaldehyde resin) and 0.708 kg of ethyl acetate while stirring. The mass ratio of ethyl isocyanate acrylate to ethyl acrylate is 4:1.

[0021] (5) Add tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and ethyl acrylate (0.354 kg) in a mass ratio of 2:1. (6) Add initiator solution, raise the temperature to 70°C, and react for 2 hours to obtain modified urea-formaldehyde resin.

[0022] Example 2 Preparation of modified urea-formaldehyde resin B On the basis of Example 1, in step (5), the mixture of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and ethyl acrylate in a mass ratio of 2:1 was completely replaced by ethyl acrylate, and the other preparation steps were the same to obtain a modified urea-formaldehyde resin B.

[0023] Example 3 Preparation of modified urea-formaldehyde resin C On the basis of Example 1, in step (5), the mixture of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and ethyl acrylate in a mass ratio of 2:1 was completely replaced by THEICTA, and the other preparation steps were the same to obtain a modified urea-formaldehyde resin C.

[0024] Example 4 Preparation of modified urea-formaldehyde resin D On the basis of Example 1, in step (4), 0.354 kg of the mixture of isocyanate ethyl acrylate and ethyl acrylate and ethyl acetate were all replaced with 0.354 kg of isocyanate ethyl acrylate, and the other preparation steps were the same to obtain modified urea-formaldehyde resin D.

[0025] Example 5 Preparation of modified urea-formaldehyde resin E On the basis of Example 1, steps (4) to (6) were omitted. At the same time, 3.54 kg of acrylic resin elastic emulsion (solid content of 20%) was added to the basic modified urea-formaldehyde resin and stirred at high speed for 20 minutes to obtain modified urea-formaldehyde resin E. Example 6 Preparation of modified urea-formaldehyde resin F On the basis of Example 1, steps (4) to (6) are omitted to directly obtain the basic modified urea-formaldehyde resin F.

[0026] Example 7 Preparation of fire retardant coating According to weight percentage, 6% of expandable vermiculite, 12% of coating additives and fillers, 24% of intumescent flame retardant, 20% of vinyl acetate-ethylene copolymer (VAE) emulsion, 20% of modified urea-formaldehyde resin and 18% of tap water are stirred in a high-speed disperser at 1000 rpm to obtain a fire retardant coating, and fire retardant coatings A, B, C, D, E, F prepared by using Examples 1-6 are obtained. Among them, the VAE emulsion is EZ 3066, the defoamer is 0.4%, the leveling agent is 0.3%, the thickener is 0.3%, the dispersant is 0.5%, the preservative is 0.5%, and the titanium dioxide is 10%. The intumescent flame retardant includes 6% pentaerythritol, 12% ammonium polyphosphate, and 6% melamine.

[0027] Fire resistance test The water-based fire retardant coating for steel structure prepared in Example 7 was sprayed on the steel plate so that the thickness of the coating was 3±0.1 mm; after 12 hours of surface drying, the fire resistance limit of the coating was tested with reference to the test method for thermal insulation efficiency deviation described in GB14907-2018, and the fire resistance limit of the water-based fire retardant coating for steel structure prepared in Example 7 was tested, and the test results are shown in Table 1. The coating of this embodiment was tested according to the standard GB 14907-2018 "Fire Retardant Coating for Steel Structure", and the results are shown in Table 1.

[0028] Water resistance test According to GB14907-2018 standard, the edge of the specimen is sealed with a molten mixture of paraffin and rosin (mass ratio is 1:1), and the edge width shall not be less than 5mm. After the mixture is completely solidified, it shall continue to be cured for 24 hours; during the test, all the specimens shall be immersed in a container filled with tap water. During the experiment, the appearance of the fire retardant coating on the surface of the specimen should be observed and recorded until the specified test time (24h) is reached. At the same time, in order to compare the differences in water resistance of different coatings, the time when the coating appears to be delaminated, foamed, and detached is recorded.

[0029] Table 1 Fire resistance and water resistance test of fire retardant coating coating Refractory time / min Water resistance (》24-hour water immersion test with no delamination, blistering or shedding of the coating) Evaluation of strength, uniformity and adhesion of carbon foam layer Fire retardant coating A 152 Qualified (28 hours) High strength and uniformity Fire retardant coating B 122 Qualified (28 hours) High strength and uniformity Fire retardant coating C 131 Qualified (28 hours) High strength and uniformity Fire retardant coating D 135 Qualified (27h) High strength and uniformity Fire retardant coating E 102 24h coating starts to fall off (12 hours) Average strength, uneven, easy to fall off Fire retardant coating F 121 24h coating peeling off (8 hours) Average strength, uneven, easy to fall off It can be seen from Table 1 that the water-based ultra-thin intumescent steel structure fire retardant coating of the present invention has good fire resistance and water resistance.

Claims

1. A fire retardant coating, characterized in that: The invention comprises the following components in weight percentage: 10-30% of vinyl acetate-ethylene copolymer (VAE) emulsion, 10-30% of modified urea-formaldehyde resin, 5-20% of expandable vermiculite, 10-30% of coating additives and other fillers, 10-30% of intumescent flame retardant, and 5-30% of water; wherein the modified urea-formaldehyde resin is obtained by chemically coating and modifying melamine-modified urea-formaldehyde resin with polyacrylate; The intumescent flame retardant is composed of a low molecular carbon source, a carbon-forming catalyst and a foaming agent, the low molecular carbon source is pentaerythritol, dipentaerythritol or tripentaerythritol, the carbon-forming catalyst is ammonium polyphosphate, diammonium phosphate, monoammonium phosphate, ammonium metaphosphate, ammonium hypophosphite, ammonium phosphite, phosphorous acid, metaphosphoric acid and / or orthophosphoric acid, and the foaming agent is melamine, dicyandiamide, ammonium oxalate, urea or hexamethylenetetramine; wherein, in terms of mass ratio, the weight ratio of the low molecular carbon source, the carbon-forming catalyst and the foaming agent is (1-2):(1-2):(0.5-1.5); Coating additives include defoamers, leveling agents, dispersants, thickeners and / or wetting agents; Other fillers include titanium dioxide.

2. The fire retardant coating according to claim 1, wherein the manufacturing process of the modified urea-formaldehyde resin is prepared by an alkali-acid-alkali process, specifically comprising the following steps: (1) Add a certain mass of formaldehyde solution into the reactor, add a certain amount of deionized water, then adjust the pH to 7.5-9.0 with sodium hydroxide aqueous solution, and heat to 40-55°C, then add the first batch of urea and the first batch of melamine under stirring conditions, heat to 85-95°C and keep the temperature for 20-40 minutes or heat to 70-75°C and keep the temperature for 50-80 minutes; (2) Adjust the pH to 5.0-5.5 with formic acid, raise the temperature to 80-95°C, continue to keep the temperature for a period of time, and finally cool the reactants to 65-75°C, adjust the pH to 7.0-7.5 with sodium hydroxide aqueous solution, add the second batch of urea and the second batch of melamine, stir evenly, and keep the temperature for 20-40 minutes; (3) After cooling to a certain temperature, add the third batch of urea, keep the temperature at 70-90°C for 10-40 minutes, and then adjust the pH value to 8.0-9.0 to obtain a basic modified urea-formaldehyde resin; (4) adding the pre-prepared mixture of isocyanate acrylate, acrylate and ester solvent while stirring, and reacting for 15-25 minutes; wherein, Based on the basic modified urea-formaldehyde resin, the sum of the amounts of isocyanate acrylate and acrylate is 5-10wt%; (5) adding 5-10 wt% of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and acrylate mixture based on the basic modified urea-formaldehyde resin while stirring, the mass ratio of the two being (2-4):1; (6) Add initiator solution, raise the temperature to 50-90°C, and react for 0.4-3.5 hours to obtain modified urea-formaldehyde resin.

3. The fire retardant coating according to claim 2, characterized in that: In steps (1) to (3), the cumulative molar ratio of formaldehyde / (urea+melamine) is 1.05-1.

15.

4. The fire retardant coating according to claim 2, characterized in that: In step (2), the reaction was continued at a temperature of 16 to 20 seconds until the viscosity of the system reached 16 to 20 seconds, and then the reactants were cooled to 65 to 75°C. The test conditions were 30°C and the coating-4 cup test was used.

5. The fire retardant coating according to claim 2, characterized in that: In step (4), the weight ratio of isocyanate acrylate to acrylate is (3-5):

1.

6. The fire retardant coating according to claim 2, characterized in that: The isocyanate acrylate is isocyanate ethyl acrylate or isocyanate ethyl methacrylate.

7. The fire retardant coating according to claim 2, characterized in that: The ester solvent in step (4) includes one or more of ethyl acetate, octyl acetate, and n-butyl acetate.

8. The fire retardant coating according to claim 2, characterized in that: The acrylic acid ester in step (4) can be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate.

9. The fire retardant coating according to claim 2, characterized in that: The acrylate in step (5) can be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate.

10. The fire retardant coating according to claim 2, characterized in that: In step (6), the initiator is one or more of sodium persulfate, azobisisobutyronitrile, dibenzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, diisopropylbenzene peroxide, and di-tert-amyl peroxide.

Citation Information

Patent Citations

  • Preparation method of modified urea-formaldehyde resin with improved storage stability

    CN102898604A

  • Multifunctional water-based paint and preparation method thereof

    CN114213912A

  • Room-temperature self-repairing water-based transparent expansion fireproof coating and preparation method thereof

    CN114250023A

  • Waterborne ultra-thin steel structure fire retardant coating and preparation method thereof

    CN102838907A

  • Expansive waterborne fireproof and flame-retardant coating for wood material and preparation method of expansive waterborne fireproof and flame-retardant coating

    CN109370288A