Ultralow-temperature curing powder coating as well as preparation device and method
By using unsaturated polyester resin, vinyl ether urethane crosslinker and other components and preparation devices in powder coatings, rapid curing is achieved at low temperatures, and the wood deformation problem caused by high-temperature curing of traditional powder coatings is solved. It improves the physical performance and service life of the product and reduces the energy consumption of the coating.
Patent Information
- Application Number
- CN202411115626.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional powder coatings may cause wood moisture evaporation, increase internal pressure, structural deformation and cracking during high-temperature curing, affecting product quality and service life.
Using ultra-low temperature curing powder coating formula, including unsaturated polyester resin, vinyl ether urethane crosslinking agent, photoinitiator, thermal initiator and additive, reduce curing through carefully selected raw material ratios and preparation processes. Temperature, using the collaborative work of extrusion, tableting, crushing and grinding components to prepare powder coatings that can cure quickly below 85-95°C.
It realizes rapid curing of powder coatings, provides excellent physical properties and weather resistance, reduces coating energy consumption, avoids the thermal expansion and contraction effect of wood, and improves the appearance quality and service life of the product.
Smart Images

Figure CN118931336A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coating preparation, and in particular to an ultra-low temperature curing powder coating, a preparation device and a preparation method. Background Art
[0002] At present, most of the powder coatings used for wood coating on the market adopt saturated epoxy / polyester hybrid formula. This type of powder coating is widely used in furniture manufacturing and other wood products industries due to its good physical properties and chemical stability. The traditional curing process usually relies on infrared radiation heating, which requires the wood surface temperature to reach about 130°C and maintain it for 3 to 5 minutes to complete the curing process.
[0003] However, for a natural material like wood, a high temperature of 130°C may cause a series of problems. First, the moisture in the wood may evaporate rapidly due to the high temperature, causing internal pressure to increase and form bubbles. Second, the wood structure may deform or even crack due to the thermal expansion and contraction effect. These factors not only affect the appearance quality of the final product, but may also reduce its service life. Summary of the invention
[0004] The object of the present invention is to provide an ultra-low temperature curing powder coating, a preparation device and a method, so as to reduce the curing temperature and achieve better use effect.
[0005] To achieve the above objectives, in the first aspect, the present invention provides an ultra-low temperature curing powder coating, which is composed of the following components by weight: 50-70 parts of unsaturated polyester resin, 20-30 parts of vinyl ether urethane crosslinker, 1-5 parts of photosensitive initiator, 1-5 parts of thermal initiator, and 5-10 parts of auxiliary agent.
[0006] The auxiliary agents include non-silicon leveling agents, silicon oxide matting agents and ultraviolet absorbers.
[0007] In a second aspect, the present invention further provides a method for preparing an ultra-low temperature curing powder coating, comprising:
[0008] Unsaturated polyester resin, vinyl ether urethane crosslinking agent, photosensitive initiator, thermal initiator and auxiliary agent are weighed according to the proportion, and placed in a mixing assembly for thorough mixing to obtain a premixed material;
[0009] Setting the extrusion temperature of the extrusion component, feeding the premixed material into the extrusion component for extrusion;
[0010] The material after discharge is compressed into tablets by a tablet press and cooled;
[0011] The cooled material is crushed and ground by a crushing assembly to obtain an ultra-low temperature curing powder coating.
[0012] In the third aspect, the present invention also provides a preparation device for ultra-low temperature curing powder coating, comprising a mixing component, an extrusion component, a tabletting cooling component and a crushing component, the crushing component comprising a supporting structure, a crushing structure and a grinding structure, the supporting structure comprising a base, a supporting frame, a crushing shell and a feed plate, the supporting frame is fixedly connected to the base and is located at the bottom of the base, the crushing shell is arranged on the supporting frame, and the feed plate is arranged at the feed port of the crushing shell, the crushing component comprises two crushing rollers, a driving motor, a driven wheel and a driving wheel, the two crushing rollers are rotatably arranged on the crushing shell, the driving wheel and the driven wheel are respectively fixed on the two crushing rollers and mesh with each other, and the output end of the driving motor is connected to the driving wheel; the grinding component comprises a supporting disc, a grinding disc and a second motor, the supporting disc is fixed in the crushing shell, the grinding disc has a feed port, the grinding disc is rotatably arranged on the supporting disc, and the output end of the second motor is connected to the grinding disc.
[0013] Wherein, the feed plate includes a plate body, a supporting spring, a feed roller and a feed motor, the plate body is rotatably arranged on the top of the crushing shell, the supporting spring is arranged between the plate body and the crushing shell, the feed roller is rotatably arranged on the support frame and is located on one side of the plate body, and the output end of the feed motor is connected to the feed roller.
[0014] Wherein, the crushing assembly further comprises two material guide plates, and the two material guide plates are located between the crushing roller and the grinding disc.
[0015] Wherein, the grinding assembly also includes a supporting cone, a screening box, a rotating rod, a third motor and a scraper rod, the supporting cone is arranged around the supporting plate, the third motor is fixed at the bottom of the supporting plate, the rotating rod is connected to the output end of the third motor, the scraper rod is arranged at the end of the rotating rod and contacts the supporting cone, the screening box is fixedly connected to the rotating rod and is located on one side of the scraper rod.
[0016] Wherein, the screening box comprises a box body, an inclined screen plate and a baffle, the inclined screen plate is arranged in the box body, and the baffle is rotatably arranged on one side of the box body.
[0017] The present invention discloses an ultra-low temperature curing powder coating, a preparation device and a method, wherein the coating is composed of the following components by weight: 50-70 parts of unsaturated polyester resin, 20-30 parts of vinyl ether urethane crosslinking agent, 1-5 parts of photosensitive initiator, 1-5 parts of thermal initiator, and 5-10 parts of auxiliary agent. The ultra-low temperature curing powder coating can not only achieve rapid curing through carefully selected raw materials and their proportions, but also provide excellent physical properties and weather resistance. The problem of the irradiation distance of the light used for making special shapes by pure ultraviolet light in the unsaturated polyester system is solved, and a thermal initiator is added to assist in curing, thereby reducing the curing temperature and achieving a better use effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 The present invention is a flow chart of a method for preparing an ultra-low temperature curing powder coating according to the second embodiment of the present invention.
[0020] Figure 2 It is a structural diagram of an ultra-low temperature curing powder coating preparation device according to the third embodiment of the present invention.
[0021] Figure 3 4 is a structural diagram of a crushing assembly according to a third embodiment of the present invention.
[0022] Figure 4 It is a right side structural diagram of a crushing assembly according to a third embodiment of the present invention.
[0023] Figure 5 It is a first cross-sectional structural diagram of a crushing assembly according to a third embodiment of the present invention.
[0024] Figure 6 It is a second cross-sectional structural diagram of the crushing assembly of the third embodiment of the present invention.
[0025] Figure 7 yes Figure 6 A partial enlargement of detail A.
[0026] Figure 8 4 is a third cross-sectional structural diagram of a crushing assembly according to a third embodiment of the present invention.
[0027] Mixing component 201, extrusion component 202, tablet cooling component 203, crushing component 204, supporting structure 205, crushing structure 206, grinding structure 207, base 209, support frame 210, crushing shell 211, feed plate 212, crushing roller 213, drive motor 214, driven wheel 215, drive wheel 216, support disk 217, grinding disk 218, second motor 219, feed inlet 220, guide plate 221, supporting cone 222, screening box 223, rotating rod 224, third motor 225, scraper rod 226, box body 227, inclined screen plate 228, baffle 229, support shaft 230, scraper rod body 231, support spring 232, gear 233, gear ring 234. DETAILED DESCRIPTION
[0028] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0029] In the description of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, in the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined.
[0030] First embodiment
[0031] The invention provides an ultra-low temperature curing powder coating, which consists of the following components by weight: 50-70 parts of unsaturated polyester resin, 20-30 parts of vinyl ether urethane crosslinking agent, 1-5 parts of photosensitive initiator, 1-5 parts of thermal initiator, and 5-10 parts of auxiliary agent.
[0032] The auxiliary agent comprises a non-silicon leveling agent, a silicon oxide matting agent and an ultraviolet absorber.
[0033] This powder coating is mainly composed of the following key ingredients, which are mixed in specific weight proportions: Unsaturated polyester resin is the base resin of the coating, which provides the necessary physical properties and chemical stability for the powder coating. It also gives the coating good adhesion, weather resistance and chemical resistance. Vinyl ether urethane crosslinker (20-30 parts) can react chemically with the unsaturated polyester resin at a lower temperature to form a three-dimensional network structure, thereby enhancing the hardness, wear resistance and corrosion resistance of the coating. Because it can be cured at a lower temperature, it is particularly suitable for heat-sensitive substrates. Photoinitiators can decompose and produce free radicals under ultraviolet or visible light, promote the polymerization reaction between the resin and the crosslinker, and accelerate the curing process of the coating. This helps to improve production efficiency and reduce energy consumption. Thermosensitive initiators decompose under heating conditions to produce free radicals, further promoting the curing reaction. It works together with the photoinitiator to ensure that sufficient curing can be completed even in insufficient light. Additives are a class of additives used in coatings to improve specific properties. In this formula, the additives mainly include:
[0034] Non-silicone leveling agents help the coating surface to be smoother after coating, reduce orange peel phenomenon and improve aesthetics. Silica matting agents scatter light by forming tiny bumps on the coating surface, thereby achieving a matte effect and giving the coating a matte appearance. UV absorbers absorb harmful UV rays and convert them into harmless energy forms for release, protecting the coating from UV damage and extending its service life.
[0035] In summary, this ultra-low temperature curing powder coating can not only achieve rapid curing through carefully selected raw materials and their proportions, but also provide excellent physical properties and weather resistance. It solves the problem of the irradiation distance of pure ultraviolet light for special-shaped unsaturated polyester systems, and adds thermal initiators to assist in curing. The physical and chemical properties of the coating fully meet the physical and chemical index requirements of GB / T3324, and the curing temperature of the original epoxy polyester mixed type is reduced from 130 degrees for 3 minutes to 85-95 degrees for 1-3 minutes. The curing temperature and curing time are greatly reduced, which reduces the energy consumption of coating. This product has excellent performance and has been selected after multiple tests and optimizations. It overcomes the existing technical defects and has obvious advantages compared with products on the market. It has broad market prospects. After promotion and application, it is expected that the economic benefits of this product will be very considerable, while reducing the energy consumption of coating by 40%.
[0036] Second embodiment
[0037] See also Figure 1 On the basis of the first embodiment, the present invention further provides a method for preparing an ultra-low temperature curing powder coating, comprising:
[0038] S201: weigh unsaturated polyester resin, vinyl ether urethane crosslinking agent, photoinitiator, thermal initiator and auxiliary agent according to the proportion, and place them in a mixing assembly for thorough mixing to obtain a premixed material;
[0039] First, accurately weigh the required unsaturated polyester resin (50-70 parts), vinyl ether urethane crosslinker (20-30 parts), photoinitiator (1-5 parts), thermal initiator (1-5 parts) and auxiliary agent (5-10 parts) according to the given ratio. Put all the above raw materials into the mixing assembly and mix them thoroughly to ensure that each component is evenly dispersed in the entire mixture to form a premixed material.
[0040] S202 sets the extrusion temperature of the extrusion component, and feeds the premixed material into the extrusion component for extrusion;
[0041] According to the characteristics of the materials used, the extrusion temperature of the extrusion component is set. The temperature should be enough to melt the raw materials but not cause them to decompose. The premixed materials are fed into the extrusion component with the set temperature, and the materials are extruded into strips or other shapes through the extruder.
[0042] The material after S203 is tableted and cooled by a tablet press;
[0043] The extruded material is fed into a tablet press and pressed into a thin sheet for subsequent processing. The sheeted material is placed in a cooling device for cooling to ensure that the material hardens and maintains a stable shape for the next step.
[0044] S204 crushes and grinds the cooled free material through a crushing assembly to obtain an ultra-low temperature curing powder coating.
[0045] The cooled material is crushed into smaller particles using a crushing assembly. The crushed material is further refined by a grinding device until a powder coating of the desired particle size is obtained. The resulting powder coating is an ultra-low temperature curing powder coating that can be used in a variety of applications that require low temperature curing conditions.
[0046] Third embodiment
[0047] See also Figure 2 to Figure 8The present invention also provides a preparation device for ultra-low temperature curing powder coating, including a mixing component 201, an extrusion component 202, a tablet cooling component 203 and a crushing component 204, wherein the crushing component 204 includes a supporting structure 205, a crushing structure 206, and a grinding structure 207, wherein the supporting structure 205 includes a base 209, a support frame 210, a crushing shell 211 and a feed plate 212, wherein the support frame 210 is fixedly connected to the base 209 and is located at the bottom of the base 209, the crushing shell 211 is arranged on the support frame 210, and the feed plate 212 is arranged at the feed port 220 of the crushing shell 211, and the crushing component 204 includes two Crushing roller 213, driving motor 214, driven wheel 215 and driving wheel 216, the two crushing rollers 213 are rotatably arranged on the crushing shell 211, the driving wheel 216 and the driven wheel 215 are respectively fixed on the two crushing rollers 213 and mesh with each other, and the output end of the driving motor 214 is connected to the driving wheel 216; the grinding assembly includes a supporting plate 217, a grinding plate 218 and a second motor 219, the supporting plate 217 is fixed in the crushing shell 211, the grinding plate 218 has a feed port 220, the grinding plate 218 is rotatably arranged on the supporting plate 217, and the output end of the second motor 219 is connected to the grinding plate 218.
[0048] The mixing component 201 is used to weigh the raw materials such as unsaturated polyester resin, vinyl ether urethane crosslinking agent, photosensitive initiator, thermal initiator and auxiliary agent according to proportion and put them into the mixing component 201 for mixing. The extrusion component 202 is used to send the premixed material into the extrusion component 202 after setting the extrusion temperature, and extrude it under a certain temperature and pressure. The tableting cooling component 203 is used to send the extruded material into the tablet press to be pressed into a sheet, and then cool the sheet material to room temperature through the cooling component.
[0049] The base 209 of the crushing assembly 204 serves as the basic support part of the entire crushing assembly 204. The support frame 210 is fixedly connected to the base 209 and is used to support the crushing shell 211. The crushing shell 211 is a closed shell for accommodating the crushing structure 206. The feed plate 212 is arranged at the feed inlet 220 of the crushing shell 211, and the material enters the crushing shell 211 from here. The crushing structure 206 includes two crushing rollers 213, a driving motor 214, a driven wheel 215 and a driving wheel 216. The two crushing rollers 213 are rotatably arranged in the crushing shell 211 to crush the material. The driving motor 214 provides power, which is transmitted through the driving wheel 216 and the driven wheel 215 to drive the two crushing rollers 213 to rotate. The support plate 217 of the grinding structure 207 is fixed in the crushing shell 211 and is used to support the grinding disc 218. The grinding disc 218: has a feed inlet 220, is rotatably arranged on the support plate 217, and is used to grind the material. The second motor 219 is connected to the grinding disc 218 to provide power to rotate the grinding disc 218 .
[0050] During operation, the cooled material enters the crushing shell 211 through the feed plate 212. The drive motor 214 is started, and the two crushing rollers 213 are driven to rotate through the driven wheel 215 and the drive wheel 216. The material is crushed into smaller particles by the extrusion and shear force between the crushing rollers 213. The crushed material enters the grinding disc 218 and passes through the feed port 220. The second motor 219 is started, driving the grinding disc 218 to rotate. Under the friction between the grinding disc 218 and the support disc 217, the material is further ground into fine powder. Thereby, the preparation efficiency can be improved.
[0051] The crushing assembly 204 further includes two guide plates 221 , and the two guide plates 221 are located between the crushing roller and the grinding disc 218 .
[0052] The two guide plates 221 are located between the crushing roller 213 and the grinding disc 218 to guide the crushed materials to smoothly enter the grinding structure 207. Specifically, after the materials are crushed by the crushing roller 213, they are guided to the grinding disc 218 below through the two guide plates 221 to ensure that the materials are evenly distributed and smoothly enter the grinding stage.
[0053] The grinding assembly further includes a supporting cone 222, a sieving box 223, a rotating rod 224, a third motor 225 and a scraper 226. The supporting cone 222 is arranged around the supporting plate 217. The third motor 225 is fixed at the bottom of the supporting plate 217. The rotating rod 224 is connected to the output end of the third motor 225. The scraper 226 is arranged at the end of the rotating rod 224 and contacts the supporting cone 222. The sieving box 223 is fixedly connected to the rotating rod 224 and is located on one side of the scraper 226. The third motor 225 is started to drive the rotating rod 224 to rotate. When the rotating rod 224 rotates, it drives the sieving box 223 and the scraper 226 to rotate together. The scraper 226 can effectively scrape the material on the supporting cone 222 into the sieving box 223. The sieve in the sieving box 223 screens out the powder coating that meets the particle size requirements, while the powder that does not meet the standards is left in the sieving box 223.
[0054] The screening box includes a box body 227 , an inclined screen plate 228 and a baffle 229 . The inclined screen plate 228 is arranged in the box body 227 , and the baffle 229 is rotatably arranged on one side of the box body 227 .
[0055] The box body 227 is used to collect the powder coating after screening. The inclined screen plate 228 is arranged in the box body 227 for further screening the powder coating. It is arranged obliquely in the box body 227 so that the materials left on the inclined screen plate 228 can move to one side of the baffle plate 229 under the action of gravity. After working for a period of time, the baffle plate 229 can be opened to take out the materials that do not meet the requirements and then grind them again, thereby improving the utilization rate.
[0056] The scraper rod 226 includes a support shaft 230, multiple scraper rod bodies 231, multiple support springs 232, a gear 233 and a ring gear 234. The ring gear 234 is fixed on the supporting cone surface 222. The support shaft 230 is rotatably connected to the rotating rod 224. The gear 233 is fixedly connected to the support shaft 230 and meshes with the ring gear 234. Multiple scraper bodies are rotatably arranged around the support shaft 230. Multiple support springs 232 are used to support multiple scraper rod bodies 231.
[0057] When the rotating rod 224 rotates, the gear 233 meshes with the gear ring 234, so that the support shaft 230 can rotate smoothly. Thus, the plurality of scraper rod bodies 231 can be driven to rotate to scrape the material on the supporting cone 222. When the scraper rod body 231 contacts the box body 227, the scraper body can rotate to eliminate the interference with the box body 227. After rotating out of the box body 227, the scraper rod body 231 can be driven to return to the initial position under the action of the support spring 232, so that the plurality of scraper rod bodies 231 can continuously scrape the material.
[0058] Through the coordinated work of these components, ultra-low temperature curing powder coatings can be prepared efficiently and ensure that the quality of the powder coatings meets the requirements.
[0059] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. An ultra-low temperature curing powder coating, characterized in that: The coating is composed of the following components by weight: 50-70 parts of unsaturated polyester resin, 20-30 parts of vinyl ether urethane crosslinking agent, 1-5 parts of photosensitive initiator, 1-5 parts of thermal initiator and 5-10 parts of auxiliary agent.
2. The ultra-low temperature curing powder coating according to claim 1, characterized in that: The auxiliary agent comprises a non-silicon leveling agent, a silicon oxide matting agent and an ultraviolet absorber.
3. A method for preparing an ultra-low temperature curing powder coating, which is used to prepare an ultra-low temperature curing powder coating according to claim 1, characterized in that: include: Unsaturated polyester resin, vinyl ether urethane crosslinking agent, photosensitive initiator, thermal initiator and auxiliary agent are weighed according to the proportion, and placed in a mixing assembly for thorough mixing to obtain a premixed material; Setting the extrusion temperature of the extrusion component, feeding the premixed material into the extrusion component for extrusion; The material after discharge is compressed into tablets by a tablet press and cooled; The cooled material is crushed and ground by a crushing assembly to obtain an ultra-low temperature curing powder coating.
4. A device for preparing ultra-low temperature curing powder coating, applied to the method for preparing ultra-low temperature curing powder coating according to claim 3, comprising a mixing component, an extrusion component, and a tableting cooling component, characterized in that: It also includes a crushing assembly, which includes a supporting structure, a crushing structure, and a grinding structure. The supporting structure includes a base, a supporting frame, a crushing shell and a feed plate. The supporting frame is fixedly connected to the base and is located at the bottom of the base. The crushing shell is arranged on the supporting frame, and the feed plate is arranged at the feed port of the crushing shell. The crushing assembly includes two crushing rollers, a driving motor, a driven wheel and a driving wheel. The two crushing rollers are rotatably arranged on the crushing shell. The driving wheel and the driven wheel are respectively fixed on the two crushing rollers and mesh with each other. The output end of the driving motor is connected to the driving wheel; the grinding assembly includes a supporting disc, a grinding disc and a second motor. The supporting disc is fixed in the crushing shell. The grinding disc has a feed port. The grinding disc is rotatably arranged on the supporting disc, and the output end of the second motor is connected to the grinding disc.
5. The device for preparing ultra-low temperature curing powder coating according to claim 4, characterized in that: The feed plate includes a plate body, a supporting spring, a feed roller and a feed motor. The plate body is rotatably arranged on the top of the crushing shell, the supporting spring is arranged between the plate body and the crushing shell, the feed roller is rotatably arranged on the supporting frame and is located on one side of the plate body, and the output end of the feed motor is connected to the feed roller.
6. The device for preparing ultra-low temperature curing powder coating according to claim 5, characterized in that: The crushing assembly further comprises two guide plates, and the two guide plates are located between the crushing roller and the grinding disc.
7. The device for preparing ultra-low temperature curing powder coating according to claim 6, characterized in that: The grinding assembly also includes a supporting cone, a screening box, a rotating rod, a third motor and a scraper rod. The supporting cone is arranged around the supporting plate, the third motor is fixed to the bottom of the supporting plate, the rotating rod is connected to the output end of the third motor, the scraper rod is arranged at the end of the rotating rod and contacts the supporting cone, and the screening box is fixedly connected to the rotating rod and is located on one side of the scraper rod.
8. The device for preparing ultra-low temperature curing powder coating according to claim 7, characterized in that: The screening box comprises a box body, an inclined screen plate and a baffle, wherein the inclined screen plate is arranged in the box body, and the baffle is rotatably arranged at one side of the box body.
Citation Information
Patent Citations
High-leveling transparent woodware powder coating with curing temperature lower than boiling point of water and preparation method thereof
CN113913092A
Device for producing powder coating
CN209775472U
Grinding device for thermosetting powder coating production
CN212524282U
Colloid mill grinding device
CN219682807U
Energy-saving pulping machine capable of preventing clamping stagnation of raw materials
CN220496560U