Solvent-free acid and alkali resistant anticorrosive paint
By using silicon sol and polyurethane prepolymers in acid-alkali-resistant anticorrosion coatings, the environmental pollution and protective performance degradation caused by solvent volatility in existing coatings during construction are solved, and efficient construction of solvent-free coatings and long-term acid-alkali-resistant acid-alkali-resistant coatings are achieved. The performance meets increasingly stringent environmental protection requirements and complex use environments.
Patent Information
- Application Number
- CN202411282404.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing acid-alkali-resistant anticorrosion coatings require solvents to be added during construction, resulting in degradation of environmental pollution and protective performance. The protection effect is weakened after long-term use in acid-alkali environments, which cannot meet the long-term anticorrosion needs.
Using solvent-free acid and alkali-resistant anticorrosion coatings, by adding silicon sol and polyurethane prepolymers to the coating, a stable colloid and polymer structure is formed, which improves the viscosity, weather resistance and chemical resistance of the coating, reduces the use of solvents, and enhances coating. The flatness and protection of the membrane.
The construction of solvent-free coatings is realized, the flatness and acid- and alkali-resistant properties of the coating are improved, the service life of the coating is extended, environmental pollution and construction costs are reduced, and the water resistance and chemical resistance of the coating are enhanced.
Smart Images

Figure BDA0005042066250000111 
Figure BDA0005042066250000112 
Figure BDA0005042066250000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-corrosion coatings, in particular to a solvent-free acid- and alkali-resistant anti-corrosion coating. Background Art
[0002] In modern industry and daily life, anti-corrosion coatings play a vital role. They are widely used in metal structures, pipelines, storage tanks, ships and other fields to protect the substrate from corrosion and extend its service life. Traditional anti-corrosion coatings usually contain a large amount of organic solvents, which will evaporate into the atmosphere during the construction and drying process of the coatings, not only causing waste of resources, but also causing serious harm to the environment and human health. With the continuous improvement of environmental awareness and the increasingly stringent environmental regulations, the development of solvent-free anti-corrosion coatings has become an important development direction of the coatings industry. Acid and alkali resistant anti-corrosion coatings, as an important branch of anti-corrosion coatings, have a wide range of application needs in the chemical, petroleum, electric power and other industries. However, the existing acid and alkali resistant anti-corrosion coatings still have some significant shortcomings and deficiencies in practical applications. The existing coatings usually need to add a certain amount of solvent to adjust the viscosity and construction performance of the coatings during the construction process. The volatilization of the solvent will not only lead to a decrease in the solid content of the coating, affecting the protective performance of the coating, but also release volatile organic compounds (VOCs), causing pollution to the atmospheric environment. In addition, the volatilization of the solvent will also increase the construction cost because additional measures need to be taken to recover or treat the volatilized solvents.
[0003] In terms of acid and alkali resistance, existing anti-corrosion coatings also have certain limitations. Due to long-term immersion and erosion of the coating in an acidic and alkaline environment, chemical changes are prone to occur, resulting in structural damage to the coating and decreased protective performance. Some coatings may exhibit good acid and alkali resistance in the initial stage, but over time, their protective effect gradually weakens and cannot meet long-term corrosion protection needs. Summary of the invention
[0004] The purpose of the present invention is to provide a solvent-free acid- and alkali-resistant anti-corrosion coating to solve the problem that the existing acid- and alkali-resistant anti-corrosion coating proposed in the above background technology causes serious environmental pollution due to solvent volatilization, and at the same time has insufficient acid- and alkali-resistant performance and cannot meet the increasingly stringent environmental protection requirements and complex use environment.
[0005] To achieve the above object, the present invention provides the following technical solution: a solvent-free acid- and alkali-resistant anticorrosive coating, the coating comprising component A and component B;
[0006] The component A comprises the following raw materials in parts by weight: 18-24 parts of acid and alkali resistant epoxy resin, 12-15 parts of polyethylene pigment, 8-12 parts of silica sol, 42-63 parts of phosphorus titanium powder and 0.3-1.2 parts of anti-settling agent;
[0007] The component B comprises the following raw materials in parts by weight: 36-48 parts of polyurethane prepolymer, 2-4 parts of catalyst and 0.5-1.5 parts of curing agent;
[0008] The acid and alkali resistant epoxy resin is one of polyurethane modified epoxy resin, epoxyalkylamide modified epoxy resin or polyamide modified epoxy resin.
[0009] Preferably, the polyethylene pigment is one of a high-chlorinated polyethylene coating and an ethylene polyolefin pigment, and the silica sol is a thiamethoxam silica sol.
[0010] Preferably, the anti-settling agent is one of organic bentonite, fumed silica and polyolefin particles.
[0011] Preferably, the polyurethane prepolymer is a polyurethane prepolymer containing an NCO group.
[0012] Preferably, the catalyst is dibutyltin dilaurate.
[0013] Preferably, the curing agent is one of ethylenediamine, diethylenetriamine glycidyl ether adduct, polyphthalamide and low molecular weight polyphthalamide resin.
[0014] Preferably, the polyurethane prepolymer preparation method is as follows:
[0015] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually raise the temperature to T1 and keep the temperature to react, and measure the content of NCO groups in the reactants. When the content reaches a specified value, stop the reaction to obtain a primary polymer;
[0016] Step 2: Add 2,2-dimethylolpropionic acid and raise the temperature to T2. After the reaction is carried out until NCO reaches a specified value, continue to add a small molecule chain extender and carry out a chain extension reaction at T3 to increase the molecular weight of the prepolymer;
[0017] Step 3: naturally cool the prepolymer to T4, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0018] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify, to obtain an aqueous polyurethane dispersion, and then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add T5 under negative pressure to carry out a desolventizing reaction, to obtain a polyurethane prepolymer containing an NCO group.
[0019] Preferably, the temperature range of T1 in step 1 is 60° C. to 65° C., and the insulation reaction time range in step 1 is 1-2 h.
[0020] Preferably, the temperature range of T2 in step 2 is 75°C to 85°C, the temperature range of T3 in step 2 is 65°C to 75°C, and the temperature range of T4 in step 3 is 35°C to 45°C.
[0021] Preferably, the pressure range in step 4 is 0.04-0.07 MPa, the temperature range of T5 in step 4 is 55-65° C., and the reaction time range in step 4 is 2-3 h, and the desolvent in step 4 is acetone.
[0022] Compared with the prior art, the invention has the following beneficial effects: the solvent-free acid- and alkali-resistant anticorrosive coating:
[0023] 1. By adding silica sol to the anti-corrosion coating, the silica sol can form a stable colloid, increase the viscosity and thixotropy of the coating, help eliminate the sagging phenomenon during brushing, improve the flatness and decorative effect of the paint film, and at the same time, the surface tension of silica sol is small, and it can quickly diffuse into the coating to play a role in rapid leveling, which helps to improve the surface quality of the coating film, so as to achieve the purpose of not using solvents;
[0024] 2. Further, the reinforcement effect of silica sol on the resin in the coating can improve the weather resistance, chemical resistance and flexibility of the coating, thereby improving the overall performance of the coating, allowing the coating to be better applied and ensuring the coating's tolerance to acid and alkali;
[0025] 3. By adding polyurethane prepolymer to the anti-corrosion coating, the coating can dry quickly in the curing environment and increase the strength, water resistance and chemical resistance of the coating, making the coating more adaptable. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The present invention provides a technical solution: a solvent-free acid- and alkali-resistant anticorrosive coating: the coating comprises component A and component B;
[0028] Component A comprises the following raw materials in parts by weight: 18-24 parts of acid and alkali resistant epoxy resin, 12-15 parts of polyethylene pigment, 8-12 parts of silica sol, 42-63 parts of phosphorus titanium powder and 0.3-1.2 parts of anti-settling agent;
[0029] Component B comprises the following raw materials in parts by weight: 36-48 parts of polyurethane prepolymer, 2-4 parts of catalyst and 0.5-1.5 parts of curing agent;
[0030] The acid and alkali resistant epoxy resin is one of polyurethane modified epoxy resin, epoxyalkylamide modified epoxy resin or polyamide modified epoxy resin.
[0031] The polyethylene pigment is one of high chlorinated polyethylene paint and ethylene polyene pigment, and the silica sol is turpentine silica sol.
[0032] The anti-settling agent is one of organic bentonite, fumed silica and polyolefin particles.
[0033] The polyurethane prepolymer is a polyurethane prepolymer containing an NCO group.
[0034] The catalyst is dibutyltin dilaurate.
[0035] The curing agent is one of ethylenediamine, diethylenetriamine glycidyl ether adduct, polyphthalamide and low molecular weight polyphthalamide resin.
[0036] The preparation method of polyurethane prepolymer is as follows:
[0037] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually raise the temperature to T1 and keep the temperature to react, and measure the content of NCO groups in the reactants. When the content reaches a specified value, stop the reaction to obtain a primary polymer;
[0038] Step 2: Add 2,2-dimethylolpropionic acid and raise the temperature to T2. After the reaction is carried out until NCO reaches a specified value, continue to add a small molecule chain extender and carry out a chain extension reaction at T3 to increase the molecular weight of the prepolymer;
[0039] Step 3: naturally cool the prepolymer to T4, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0040] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify, to obtain an aqueous polyurethane dispersion, and then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add T5 under negative pressure to carry out a desolventizing reaction, to obtain a polyurethane prepolymer containing an NCO group.
[0041] The temperature range of T1 in step 1 is 60° C. to 65° C., and the insulation reaction time range in step 1 is 1-2 h.
[0042] The temperature range of T2 in step 2 is 75°C to 85°C, the temperature range of T3 in step 2 is 65°C to 75°C, and the temperature range of T4 in step 3 is 35°C to 45°C.
[0043] The pressure range in step 4 is 0.04-0.07 MPa, the temperature range of T5 in step 4 is 55-65°C, the reaction time range in step 4 is 2-3h, and the solvent removed in step 4 is acetone
[0044] Example 1, this example discloses: Component A comprises the following raw materials in parts by weight: 18 parts of polyurethane modified epoxy resin, 12 parts of high chlorinated polyethylene coating, 8 parts of guar peptide silica sol, 42 parts of phosphorus titanium powder and 0.3 parts of organic bentonite;
[0045] Component B comprises the following raw materials in parts by weight: 36 parts of polyurethane prepolymer containing NCO group, 2 parts of triethanolamine and 0.5 parts of ethylenediamine;
[0046] The preparation method of polyurethane prepolymer is as follows:
[0047] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually heat to 60°C and keep warm for 1.5 hours, and measure the content of NCO groups in the reactants. When the content reaches the specified value, stop the reaction to obtain a primary polymer;
[0048] Step 2: Add 2,2-dimethylolpropionic acid and heat to 80°C, react until NCO reaches a specified value, then continue to add a small molecule chain extender and carry out a chain extension reaction at 70°C to increase the molecular weight of the prepolymer;
[0049] Step 3: naturally cool the prepolymer to 40°C, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0050] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify to obtain an aqueous polyurethane dispersion, then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add acetone at 0.06 MPa and 60°C to react to obtain a polyurethane prepolymer containing an NCO group.
[0051] Example 2, this example discloses: Component A comprises the following raw materials in parts by weight: 22 parts of epoxyalkylamide modified epoxy resin, 12 parts of highly chlorinated polyethylene coating, 8 parts of guar peptide silica sol, 42 parts of phosphorus titanium powder and 0.3 parts of organic bentonite;
[0052] Component B comprises the following raw materials in parts by weight: 36 parts of polyurethane prepolymer containing NCO group, 2 parts of triethanolamine and 0.5 parts of ethylenediamine;
[0053] The preparation method of polyurethane prepolymer is as follows:
[0054] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually heat to 65°C and keep warm for 1 hour, and measure the content of NCO groups in the reactants. When the content reaches the specified value, stop the reaction to obtain a primary polymer;
[0055] Step 2: Add 2,2-dimethylolpropionic acid and heat to 75°C. After the reaction is carried out until NCO reaches a specified value, continue to add a small molecule chain extender and carry out a chain extension reaction at 75°C to increase the molecular weight of the prepolymer;
[0056] Step 3: naturally cool the prepolymer to 35°C, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0057] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify to obtain an aqueous polyurethane dispersion, then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add acetone at 0.06 MPa and 60°C to react to obtain a polyurethane prepolymer containing an NCO group.
[0058] Example 3, this example discloses: Component A comprises the following raw materials in parts by weight: 24 parts of polyamide modified epoxy resin, 12 parts of high chlorinated polyethylene coating, 8 parts of guar peptide silica sol, 42 parts of phosphorus titanium powder and 0.3 parts of organic bentonite;
[0059] Component B comprises the following raw materials in parts by weight: 36 parts of polyurethane prepolymer containing NCO group, 2 parts of triethanolamine and 0.5 parts of ethylenediamine;
[0060] The preparation method of polyurethane prepolymer is as follows:
[0061] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually heat to 60°C and keep warm for 1.5 hours, and measure the content of NCO groups in the reactants. When the content reaches the specified value, stop the reaction to obtain a primary polymer;
[0062] Step 2: Add 2,2-dimethylolpropionic acid and heat to 80°C, react until NCO reaches a specified value, then continue to add a small molecule chain extender and carry out a chain extension reaction at 70°C to increase the molecular weight of the prepolymer;
[0063] Step 3: naturally cool the prepolymer to 40°C, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0064] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify to obtain an aqueous polyurethane dispersion, then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add acetone at 0.06 MPa and 60°C to react to obtain a polyurethane prepolymer containing an NCO group.
[0065] Example 4, this example discloses: Component A comprises the following raw materials in parts by weight: 18 parts of polyurethane modified epoxy resin, 15 parts of ethylene polyolefin pigment, 8 parts of guar peptide silica sol, 42 parts of phosphorus titanium powder and 0.3 parts of organic bentonite;
[0066] Component B comprises the following raw materials in parts by weight: 36 parts of polyurethane prepolymer containing NCO group, 2 parts of triethanolamine and 0.5 parts of ethylenediamine;
[0067] The preparation method of polyurethane prepolymer is as follows:
[0068] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually heat to 65°C and keep warm for 2 hours, and measure the content of NCO groups in the reactants. When the content reaches the specified value, stop the reaction to obtain a primary polymer;
[0069] Step 2: Add 2,2-dimethylolpropionic acid and heat to 85°C. After the reaction is carried out until the NCO reaches the specified value, continue to add a small molecule chain extender and carry out a chain extension reaction at 75°C to increase the molecular weight of the prepolymer;
[0070] Step 3: naturally cool the prepolymer to 45°C, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0071] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify to obtain an aqueous polyurethane dispersion, then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add acetone at 0.04 MPa and 55°C to react to obtain a polyurethane prepolymer containing an NCO group.
[0072] Example 5. This example discloses: Component A comprises the following raw materials in parts by weight: 18 parts of polyurethane modified epoxy resin, 12 parts of high chlorinated polyethylene coating, 8 parts of guar peptide silica sol, 42 parts of phosphorus titanium powder and 0.8 parts of fumed silica;
[0073] Component B comprises the following raw materials in parts by weight: 36 parts of polyurethane prepolymer containing NCO group, 2 parts of triethanolamine and 0.5 parts of ethylenediamine;
[0074] The preparation method of polyurethane prepolymer is as follows:
[0075] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually heat to 60°C and keep warm for 1.5 hours, and measure the content of NCO groups in the reactants. When the content reaches the specified value, stop the reaction to obtain a primary polymer;
[0076] Step 2: Add 2,2-dimethylolpropionic acid and heat to 80°C, react until NCO reaches a specified value, then continue to add a small molecule chain extender and carry out a chain extension reaction at 70°C to increase the molecular weight of the prepolymer;
[0077] Step 3: naturally cool the prepolymer to 40°C, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0078] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify to obtain an aqueous polyurethane dispersion, then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add acetone at 0.06 MPa and 60°C to react to obtain a polyurethane prepolymer containing an NCO group.
[0079] Example 6. This example discloses: Component A comprises the following raw materials in parts by weight: 18 parts of polyurethane modified epoxy resin, 12 parts of high chlorinated polyethylene coating, 8 parts of turmeric peptide silica sol, 42 parts of phosphorus titanium powder and 1.2 parts of polyolefin particles;
[0080] Component B comprises the following raw materials in parts by weight: 36 parts of polyurethane prepolymer containing NCO group, 2 parts of triethanolamine and 0.5 parts of ethylenediamine;
[0081] The preparation method of polyurethane prepolymer is as follows:
[0082] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually heat to 60°C and keep warm for 1.5 hours, and measure the content of NCO groups in the reactants. When the content reaches the specified value, stop the reaction to obtain a primary polymer;
[0083] Step 2: Add 2,2-dimethylolpropionic acid and heat to 80°C, react until NCO reaches a specified value, then continue to add a small molecule chain extender and carry out a chain extension reaction at 70°C to increase the molecular weight of the prepolymer;
[0084] Step 3: naturally cool the prepolymer to 40°C, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0085] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify to obtain an aqueous polyurethane dispersion, then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add acetone at 0.07 MPa and 55°C to react to obtain a polyurethane prepolymer containing an NCO group.
[0086] Example 7, this example discloses: Component A comprises the following raw materials in parts by weight: 18 parts of polyurethane modified epoxy resin, 12 parts of high chlorinated polyethylene coating, 8 parts of guar peptide silica sol, 42 parts of phosphorus titanium powder and 0.3 parts of organic bentonite;
[0087] Component B comprises the following raw materials in parts by weight: 36 parts of polyurethane prepolymer containing NCO group, 2 parts of triethanolamine and 0.9 parts of glycidyl ether diethylenetriamine adduct;
[0088] The preparation method of polyurethane prepolymer is as follows:
[0089] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually heat to 60°C and keep warm for 1.5 hours, and measure the content of NCO groups in the reactants. When the content reaches the specified value, stop the reaction to obtain a primary polymer;
[0090] Step 2: Add 2,2-dimethylolpropionic acid and heat to 80°C, react until NCO reaches a specified value, then continue to add a small molecule chain extender and carry out a chain extension reaction at 70°C to increase the molecular weight of the prepolymer;
[0091] Step 3: naturally cool the prepolymer to 40°C, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0092] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify to obtain an aqueous polyurethane dispersion, then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add acetone at 0.06 MPa and 60°C to react to obtain a polyurethane prepolymer containing an NCO group.
[0093] Embodiment 8, this embodiment discloses: Component A comprises the following raw materials in parts by weight: 18 parts of polyurethane modified epoxy resin, 12 parts of high chlorinated polyethylene coating, 8 parts of guar peptide silica sol, 42 parts of phosphorus titanium powder and 0.3 parts of organic bentonite;
[0094] Component B comprises the following raw materials in parts by weight: 36 parts of polyurethane prepolymer containing NCO group, 2 parts of triethanolamine and 1.4 parts of polyphthalamide and low molecular weight polyphthalamide resin;
[0095] The preparation method of polyurethane prepolymer is as follows:
[0096] Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually heat to 60°C and keep warm for 1.5 hours, and measure the content of NCO groups in the reactants. When the content reaches the specified value, stop the reaction to obtain a primary polymer;
[0097] Step 2: Add 2,2-dimethylolpropionic acid and heat to 80°C, react until NCO reaches a specified value, then continue to add a small molecule chain extender and carry out a chain extension reaction at 70°C to increase the molecular weight of the prepolymer;
[0098] Step 3: naturally cool the prepolymer to 40°C, add a neutralizing agent and stir rapidly to obtain an intermediate;
[0099] Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify to obtain an aqueous polyurethane dispersion, then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add acetone at 0.06 MPa and 60°C to react to obtain a polyurethane prepolymer containing an NCO group.
[0100] Table 1 - Test data of acid and alkali resistance and corrosion resistance of the inventive coating
[0101]
[0102] It can be seen from the above table that the acid and alkali resistance of Example 1 and Example 2 is better, and the corrosion resistance of Example 3 is better.
[0103] Table 2 - Test data of acid and alkali resistance and high temperature resistance of the inventive coating
[0104]
[0105] It can be seen from the above table that the high temperature resistance of Example 4 is the best, and the coating can ensure a good protective effect in a long-term high temperature environment.
[0106] Table 3 - Physical properties test data of the inventive coating
[0107]
[0108] It can be seen from the above table that the coating of Example 6 has better fineness and better film-forming quality, and is suitable for coating protection in usage scenarios where the film-forming surface has a high smoothness. The film-forming speed of Example 8 is faster, which can improve the coating quality and prevent the occurrence of sagging.
[0109] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A solvent-free acid- and alkali-resistant anticorrosive coating, characterized in that: The coating comprises component A and component B; The component A comprises the following raw materials in parts by weight: 18-24 parts of acid and alkali resistant epoxy resin, 12-15 parts of polyethylene pigment, 8-12 parts of silica sol, 42-63 parts of phosphorus titanium powder and 0.3-1.2 parts of anti-settling agent; The component B comprises the following raw materials in parts by weight: 36-48 parts of polyurethane prepolymer, 2-4 parts of catalyst and 0.5-1.5 parts of curing agent; The acid and alkali resistant epoxy resin is one of polyurethane modified epoxy resin, epoxyalkylamide modified epoxy resin or polyamide modified epoxy resin.
2. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 1, characterized in that: The polyethylene pigment is one of a high-chlorinated polyethylene coating and an ethylene polyene pigment, and the silica sol is a thiamethoxam silica sol.
3. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 1, characterized in that: The anti-settling agent is one of organic bentonite, fumed silica and polyolefin particles.
4. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 1, characterized in that: The polyurethane prepolymer is a polyurethane prepolymer containing an NCO group.
5. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 1, characterized in that: The catalyst is dibutyltin dilaurate.
6. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 1, characterized in that: The curing agent is one of ethylenediamine, glycidyl ether diethylenetriamine adduct, polyphthalamide and low molecular weight polyphthalamide resin.
7. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 4, characterized in that: The polyurethane prepolymer preparation method is as follows: Step 1: Add toluene diisocyanate and dehydrated polyether diol into a three-necked flask, gradually raise the temperature to T1 and keep the temperature to react, and measure the content of NCO groups in the reactants. When the content reaches a specified value, stop the reaction to obtain a primary polymer; Step 2: Add 2,2-dimethylolpropionic acid and raise the temperature to T2. After the reaction is carried out until the NCO reaches the specified value, continue to add a small molecule chain extender and carry out a chain extension reaction at T3 to increase the molecular weight of the prepolymer; Step 3: naturally cool the prepolymer to T4, add a neutralizing agent and stir rapidly to obtain an intermediate; Step 4: Slowly add deionized water to the intermediate while stirring at high speed to emulsify, to obtain an aqueous polyurethane dispersion, and then transfer the emulsified aqueous polyurethane to a three-necked flask with a vacuum condenser, add T5 under negative pressure to carry out a desolventizing reaction, to obtain a polyurethane prepolymer containing an NCO group.
8. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 7, characterized in that: The temperature range of T1 in step 1 is 60° C. to 65° C., and the insulation reaction time range in step 1 is 1-2 h.
9. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 7, characterized in that: The temperature range of T2 in step 2 is 75°C to 85°C, the temperature range of T3 in step 2 is 65°C to 75°C, and the temperature range of T4 in step 3 is 35°C to 45°C.
10. The solvent-free acid- and alkali-resistant anticorrosive coating according to claim 7, characterized in that: The pressure range in step 4 is 0.04-0.07 MPa, the temperature range of T5 in step 4 is 55-65° C., and the reaction time range in step 4 is 2-3 h. The desolvent in step 4 is acetone.
Citation Information
Cited By
Titanium porcelain surface heavy anti-corrosion coating and preparation method thereof
CN119859461A
Titanium porcelain surface heavy-duty anticorrosive coating and preparation method thereof