N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating and fluoride-free preparation method thereof
The hydrothermal method is used to construct the loose porous structure of N-TiO2 and superhydrophobic modification, which solves the problem of the reduction of hydrophobicity of fluorine-free superhydrophobic coating after long-term use, and realizes effective degradation and removal of pollutants under visible light. Moreover, it adopts fluorination-free modification method, which is more environmentally friendly and is suitable for self-cleaning applications of building surfaces.
Patent Information
- Application Number
- CN202411000297.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing fluorine-free superhydrophobic coatings have a reduced hydrophobicity after long-term use, and the commonly used fluorine-containing substances in the traditional hydrophobic modification process have an impact on the environment and human health, making it difficult to achieve superhydrophobicity and excellent photocatalytic properties at the same time.
N-TiO2 loose porous structure was constructed by hydrothermal method, and superhydrophobic modification was performed using stearic acid and polydimethicone to enhance the adsorption performance of the material, so that it has superhydrophobic properties and excellent under visible light irradiation The photocatalytic performance of the pollutant can be achieved independently degraded and cleared.
The prepared PDMS/STA/N-TiO2 coating has high super hydrophobicity and stability, can effectively degrade organic pollutants such as methylene blue, and is more environmentally friendly by fluorination-free modification, and is suitable for self-cleaning applications on building surfaces.
Smart Images

Figure CN118931377A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanomaterials and super-hydrophobic materials, and particularly relates to an N-doped TiO2 photocatalytic surface self-cleaning super-hydrophobic coating and a fluorine-free preparation method thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Due to the development of industrialization, the turbidity of the atmosphere has increased. After being exposed to wind and rain, pollutants in the atmosphere are easily deposited on the surface of outdoor walls and glass to form dirt, which reduces the aesthetics and light transmittance of the glass. Therefore, the research and development of self-cleaning materials with super-hydrophobic function has become a hot topic of widespread concern.
[0004] Photocatalytic oxidation technology has become a process method that is currently being studied more for pollutant control due to its advantages such as high efficiency, low cost and green environmental protection. On the surface of traditional hydrophobic coatings, it is inevitable that some pollutants will remain. In order to effectively degrade the pollutants remaining on the surface, adding photocatalytic materials to the coating materials is an effective way. As G. Yamauchi discovered, adding a small amount of TiO2 powder to the super-hydrophobic transparent coating to improve the durability of the super-hydrophobic surface can make the coating have excellent self-cleaning properties, and enable the coating to function for a long time, and can maintain super-hydrophobicity for a long time when used outdoors.
[0005] However, in the traditional hydrophobic modification process, fluorine-containing substances are often used, which have a great impact on the environment and human health. Nowadays, some scientific researchers are committed to the research and development of fluorine-free super-hydrophobic coatings to enable green production and application of super-hydrophobic coatings, and the fluorine-free super-hydrophobic coatings prepared by the prior art often have a large gap in super-hydrophobic performance compared with fluorine-containing super-hydrophobic coatings. Therefore, the preparation of fluorine-free super-hydrophobic coatings that meet the current green environmental protection requirements is a key issue that needs to be solved urgently.
[0006] At the same time, the performance of the super-hydrophobic surface is mainly determined by the surface microstructure of the super-hydrophobicity. In long-term outdoor use, as the outdoor use time increases, the contact angle between many super-hydrophobic surfaces and water decreases, resulting in a significant reduction in hydrophobicity. Therefore, it is a technical problem that those skilled in the art need to solve urgently to develop a new type of fluorinated super-hydrophobic material, increase the contact angle between the super-hydrophobic surface and water, and then make the material have both super-hydrophobicity and excellent photocatalytic performance, and can autonomously degrade and remove pollutants. Summary of the invention
[0007] In order to solve the above technical problems, the present invention aims to provide a N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating and a fluorine-free preparation method thereof. The N-TiO2 loose porous structure is constructed by a hydrothermal method to enhance the adsorption performance of the material, and N-TiO2 is super-hydrophobically modified using stearic acid (STA) and polydimethylsiloxane (PDMS). Under visible light irradiation, the material has both super-hydrophobicity and excellent photocatalytic performance, thereby achieving autonomous degradation and removal of pollutants.
[0008] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0009] In a first aspect of the present invention, a fluorination-free preparation method of a N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating is provided, comprising the following steps:
[0010] S1, adding urea to a solution of methanol, tetrabutyl titanate and acetylacetone and performing ultrasonic treatment;
[0011] S2, mixing the reaction solution obtained in step S1 with anhydrous ethanol uniformly, and then performing hydrothermal reaction and centrifugal washing in sequence;
[0012] S3, drying, grinding and calcining the material obtained in step S2 in sequence to obtain a loose and porous N-TiO2 material;
[0013] S4, dissolving the N-TiO2 material in an organic solvent, adding stearic acid for hydrophobic modification after ultrasonic treatment, and then centrifugally washing, drying and grinding in sequence to obtain STA / N-TiO2 material;
[0014] S5. Disperse STA / N-TiO2 material and polydimethylsiloxane in ethyl acetate, then apply them on a glass slide, and obtain a PDMS / STA / N-TiO2 coating after curing.
[0015] Preferably, in step S1, the mass ratio of methanol, tetrabutyl titanate and acetylacetone is 13:3:1 to 13:3.4:1. More preferably, the mass ratio of methanol, tetrabutyl titanate and acetylacetone is 13:3.2:1.
[0016] Preferably, in step S2, the reaction temperature of the hydrothermal reaction is 180-240° C., and the reaction time is 3-6 hours.
[0017] Further preferably, the reaction temperature of the hydrothermal reaction is 220° C. and the reaction time is 5 h.
[0018] Preferably, in step S2, the organic solvent is ethanol; the specific steps of the centrifugal washing are: washing 2 to 3 times at a rate of 4300 to 5500 r / s and 2 to 4 min / time.
[0019] Further preferably, in step S2, the specific steps of the centrifugal washing are: washing three times at a rate of 5000 r / s, 3 min / time.
[0020] Preferably, in step S3, the drying temperature is 80-110° C., and the drying time is 10-13 hours.
[0021] Further preferably, in step S3, the drying temperature is 100° C. and the drying time is 12 h.
[0022] Preferably, in step S3, the calcination is carried out by heating the temperature to 450-550° C. at a heating rate of 1-3° C. / min, and the holding time is 2.5-3.5 h.
[0023] Further preferably, in step S3, the calcination is carried out by heating the temperature to 500° C. at a heating rate of 2° C. / min and keeping the temperature for 3 h.
[0024] Preferably, in step S4, the mass ratio of N-TiO2 to stearic acid is 1:1.1 to 1:1.3.
[0025] Further preferably, in step S4, the mass ratio of N-TiO2 to stearic acid is 1:1.2.
[0026] Preferably, in step S4, the temperature of the hydrophobic modification is 65-75° C. and the time is 2-3.5 h.
[0027] Further preferably, in step S4, the temperature of the hydrophobic modification is 70° C. and the time is 3 hours.
[0028] Preferably, in step S4, the drying temperature is 75-85° C. and the drying time is 6-10 hours.
[0029] Further preferably, in step S4, the drying temperature is 80° C. and the drying time is 8 hours.
[0030] Preferably, in step S5, the mass ratio of STA / N-TiO2 to polydimethylsiloxane is 1:1 to 3:2.
[0031] Further preferably, in step S5, the mass ratio of STA / N-TiO2 to polydimethylsiloxane is 5:4.
[0032] Preferably, in step S5, the specific method of coating is: after the glass slide is polished, cleaned and dried, the dispersion is sprayed at a distance of about 15 cm from the glass slide.
[0033] Preferably, in step S5, the curing temperature is 90-110° C., and the curing time is 22-25 hours.
[0034] Further preferably, in step S5, the curing temperature is 100° C. and the curing time is 24 hours.
[0035] The second aspect of the present invention provides an N-TiO2 photocatalytic surface self-cleaning super hydrophobic coating material prepared by the above method.
[0036] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:
[0037] (1) The preparation method provided by the present invention is simple and easy to control. The prepared PDMS / STA / N-TiO2 coating has a super-hydrophobic surface with a large contact angle with water, strong super-hydrophobicity, good stability, self-cleaning ability, and can effectively degrade organic pollutants such as methylene blue dye under visible light.
[0038] (2) The present invention adopts a non-fluorinated modification method, which is more environmentally friendly and has better practical feasibility. It can be widely used for spraying on glass or wall surfaces to achieve self-cleaning of the surface of buildings and other external surfaces. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Infrared spectra of N-TiO2 with different nitrogen doping amounts prepared in Examples 1-3 of the present invention and the TiO2 material prepared in Comparative Example 1.
[0040] Figure 2 XRD patterns of N-TiO2 with different nitrogen doping amounts prepared in Examples 1-3 of the present invention and the TiO2 material prepared in Comparative Example 1.
[0041] Figure 3 This is a diagram of the photocatalytic degradation efficiency of methylene blue of N-TiO2 with different nitrogen doping amounts prepared by a hydrothermal method in Examples 1-3 of the present invention, TiO2 prepared by a hydrothermal method in Comparative Example 1, and 3N-TiO2 prepared by a sol-gel method in Comparative Example 2.
[0042] Figure 4 This is a diagram showing the photocatalytic degradation efficiency of methylene blue of the 3N-TiO2 material prepared in Example 1 of the present invention at different dosages.
[0043] Figure 5 This is a diagram showing the photocatalytic degradation efficiency of methylene blue at different dosages of the 2N-TiO2 material prepared in Example 2 of the present invention.
[0044] Figure 6 This is a diagram showing the photocatalytic degradation efficiency of methylene blue at different dosages of the 4N-TiO2 material prepared in Example 3 of the present invention.
[0045] Figure 7These are the hydrophobic angle test diagrams of PDMS / STA / N-TiO2 coatings, where (a) is the PDMS / STA / 3N-TiO2 coating, (b) is the PDMS / STA / 2N-TiO2 coating, (c) is the PDMS / STA / 4N-TiO2 coating, (d) is the PDMS / STA / TiO2 coating, (e) is the PDMS / STA / 3N-TiO2 coating after two weeks of outdoor exposure experiment, and (f) is the PDMS / STA / 3N-TiO2(R) coating. DETAILED DESCRIPTION
[0046] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0047] The instruments and reagents used in the present invention are as follows:
[0048] Table 1 Instruments and equipment
[0049]
[0050]
[0051] Table 2 Main reagents
[0052]
[0053] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are intended to explain the present invention rather than to limit it.
[0054] Example 1 :
[0055] This embodiment provides a fluorination-free preparation method of a N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating material, comprising the following steps:
[0056] S1. 40 mL of methanol, 8 g of tetrabutyl titanate and 2.5 g of acetylacetone were magnetically stirred at room temperature for 30 min. 3 g of urea was weighed and added to the obtained solution, and ultrasonically treated at room temperature for 30 min;
[0057] S2. Mix the solution and anhydrous ethanol evenly, transfer to a polytetrafluoroethylene reactor, and perform hydrothermal reaction in an oven at 220°C for 5 hours. After naturally cooling to room temperature, take out the material and wash it three times by centrifugation with anhydrous ethanol (5000 r / s, 3 min / time);
[0058] S3, drying at 100°C for 12h, grinding, placing in a muffle furnace and calcining at 500°C for 3h (heating rate 2°C / min) to obtain a loose and porous 3N-TiO2 material;
[0059] S4, 3.7g of 3N-TiO2 was dissolved in 100mL of ethanol and ultrasonicated for 30min. 4.5g of stearic acid was added to the resulting solution and reacted at 70°C for 3h. The resulting material was then centrifuged and washed 3 times with anhydrous ethanol (5000r / s, 3min / time), dried at 80°C, and ground to obtain STA / 3N-TiO2 material;
[0060] S5. Disperse 2.5 g of STA / 3N-TiO2 material and 2 mL of polydimethylsiloxane in 15 mL of ethyl acetate, and stir the mixture magnetically for 30 min at room temperature. Grind the glass slide with 1500# sandpaper and clean it with ethanol and dry it. Then, spray the dispersion about 15 cm away from the glass slide. Finally, cure the PDMS / STA / 3N-TiO2 coating in an oven at 100°C for 24 h.
[0061] Example 2 :
[0062] This embodiment provides a fluorination-free preparation method of a N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating material, comprising the following steps:
[0063] S1. 40 mL of methanol, 8 g of tetrabutyl titanate and 2.5 g of acetylacetone were magnetically stirred at room temperature for 30 min. 2 g of urea was weighed and added to the obtained solution, and ultrasonically treated at room temperature for 30 min;
[0064] S2. Mix the solution and anhydrous ethanol evenly, transfer to a polytetrafluoroethylene reactor, and perform hydrothermal reaction in an oven at 220°C for 5 hours. After naturally cooling to room temperature, take out the material and wash it three times by centrifugation with anhydrous ethanol (5000 r / s, 3 min / time);
[0065] S3, drying at 100°C for 12h, grinding, placing in a muffle furnace and calcining at 500°C for 3h (heating rate 2°C / min) to obtain a loose and porous 2N-TiO2 material;
[0066] S4, dissolve 3.7g of 2N-TiO2 in 100mL of ethanol and ultrasonicate for 30min. Add 4.5g of stearic acid to the resulting solution and react at 70℃ for 3h. Then wash the resulting material with anhydrous ethanol by centrifugation 3 times (5000r / s, 3min / time), dry at 80℃, grind, and obtain STA / 2N-TiO2 material;
[0067] S5. Disperse 2.5 g of STA / 2N-TiO2 material and 2 mL of polydimethylsiloxane in 15 mL of ethyl acetate, and stir the mixture magnetically for 30 min at room temperature. Grind the glass slide with 1500# sandpaper and clean it with ethanol and dry it. Then, spray the dispersion about 15 cm away from the glass slide. Finally, cure the PDMS / STA / 2N-TiO2 coating in an oven at 100°C for 24 h.
[0068] Example 3 :
[0069] This embodiment provides a fluorination-free preparation method of a N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating material, comprising the following steps:
[0070] S1. 40 mL of methanol, 8 g of tetrabutyl titanate and 2.5 g of acetylacetone were magnetically stirred at room temperature for 30 min. 4 g of urea was weighed and added to the obtained solution, and ultrasonically treated at room temperature for 30 min;
[0071] S2. Mix the solution and anhydrous ethanol evenly, transfer to a polytetrafluoroethylene reactor, and perform hydrothermal reaction in an oven at 220°C for 5 hours. After naturally cooling to room temperature, take out the material and wash it three times by centrifugation with anhydrous ethanol (5000 r / s, 3 min / time);
[0072] S3, drying at 100°C for 12h, grinding, placing in a muffle furnace and calcining at 500°C for 3h (heating rate 2°C / min) to obtain a loose and porous 4N-TiO2 material;
[0073] S4, 3.7g of 4N-TiO2 was dissolved in 100mL of ethanol and ultrasonicated for 30min. 4.5g of stearic acid was added to the resulting solution and reacted at 70°C for 3h. The resulting material was then centrifuged and washed 3 times with anhydrous ethanol (5000r / s, 3min / time), dried at 80°C, and ground to obtain STA / 4N-TiO2 material;
[0074] S5. Disperse 2.5 g of STA / 4N-TiO2 material and 2 mL of polydimethylsiloxane in 15 mL of ethyl acetate, and stir the mixture magnetically for 30 min at room temperature. Grind the glass slide with 1500# sandpaper and clean it with ethanol and dry it. Then, spray the dispersion about 15 cm away from the glass slide. Finally, cure the PDMS / STA / 4N-TiO2 coating in an oven at 100°C for 24 h.
[0075] Comparative Example 1 :
[0076] The difference from Examples 1 to 3 is that this comparative example uses analytically pure TiO2 purchased from Shanghai MacLean Biochemical Technology Co., Ltd. as a nitrogen-undoped monomer to replace the N-TiO2 in the examples for comparison and testing the photocatalytic performance and super-hydrophobic performance of the coating.
[0077] Comparative Example 2 :
[0078] This embodiment provides a method for preparing 3N-TiO2(R) by a sol-gel method:
[0079] S1. Mix 40 mL of anhydrous ethanol, 8 g of tetrabutyl titanate and 1.5 mL of glacial acetic acid under magnetic stirring at room temperature for 1 h. Weigh 3 g of urea and dissolve it in 5 mL of distilled water, then add it to the obtained solution;
[0080] S2, using concentrated nitric acid to adjust the pH value until a yellow transparent sol is generated, then magnetically stirring for 2 hours, and standing until the sol appears;
[0081] S3. The obtained gel was dried in an oven at 100° C. for 4 h, then placed in a muffle furnace and calcined at 500° C. for 2 h (heating rate 5° C. / min) to obtain 3N-TiO2(R) material.
[0082] Example 4 :
[0083] Fourier infrared imaging tests were performed on the N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating materials with different nitrogen doping amounts obtained in Examples 1-3 and the nitrogen-free monomer TiO2 obtained in Comparative Example 1.
[0084] The results are as follows Figure 1 As shown, at 400~700cm -1 The absorption peak at 1045 cm-1 is derived from the Ti-O bond in the catalyst. -1 An absorption peak appears, which is due to the presence of O-Ti-N bonds in the N-TiO2 sample, indicating that there is nitrogen in the prepared catalyst and that nitrogen is effectively combined with TiO2. -1 The absorption peak that appears is the stretching vibration absorption peak of the OH bond, which originates from the water molecules present in the sample.
[0085] Example 5 :
[0086] XRD test was performed on the N-TiO2 photocatalytic materials with different nitrogen doping amounts obtained in Examples 1-3 and the nitrogen-free monomer TiO2 obtained in Comparative Example 1.
[0087] The results are as follows Figure 2As shown, compared with the standard card (PDF#04-005-4859), it is known that the N-TiO2 obtained in this experiment is anatase. Through further observation, the diffraction peak of the sample is sharp, and the prepared nitrogen-doped titanium dioxide sample has a high degree of crystallinity.
[0088] Example 6 :
[0089] In this example, methylene blue (MB) organic dye was used to simulate organic pollutants, and the photocatalytic degradation performance of the N-TiO2 photocatalytic surface self-cleaning super hydrophobic coating materials with different nitrogen doping amounts obtained in Examples 1-3, the nitrogen-undoped monomer TiO2 obtained in Comparative Example 1, and the 3N-TiO2 (R) material prepared by the sol-gel method in Comparative Example 2 were tested.
[0090] 100 mL of 20 ppm MB solution was added to a beaker, and the materials prepared in Examples 1-3 and Comparative Examples 1 and 2 were respectively placed in the above solutions in different beakers and stirred for 30 min to achieve stability and adsorption equilibrium. The above mixture was irradiated with full light of a xenon lamp, and the MB solution was collected every 0.5 h. The absorbance of the MB solution was measured after filtering through a filter head. The degradation efficiency was calculated by formula (I). Finally, the degradation of the dye was determined by ultraviolet spectrophotometry.
[0091] D%=(C0-C) / C0×100%Formula (I)
[0092] Where D is the degradation rate, C0 is the absorbance value at the beginning, and C is the average absorbance value at different sampling times.
[0093] The results are as follows Figure 3 As shown in the figure, compared with the pure TiO2 catalyst, the N-TiO2 doped with nitrogen has a better degradation efficiency after 120 minutes of degradation of methylene blue. Among them, the catalytic effect of 3N-TiO2 synthesized by hydrothermal method is worse than that of 3N-TiO2(R) prepared by sol-gel method. This may be because the operation process of sol-gel method is not easy to control, resulting in the nitrogen doping effect not as good as that of hydrothermal method, which in turn affects the photocatalytic efficiency. The 3N-TiO2 catalyst prepared by hydrothermal method has the best degradation effect on methylene blue, and the degradation efficiency can reach 91.32% within 120 minutes.
[0094] Example 7 :
[0095] In this example, methylene blue (MB) organic dye was used to simulate organic pollutants to evaluate the photocatalytic degradation performance of the STA / 3N-TiO2 coating at different dosages.
[0096] 100 mL of 20 ppm MB solution was added to a beaker, and the STA / nN-TiO2 coating material was placed in the solution and stirred for 30 minutes to achieve stability and adsorption equilibrium. The mixture was irradiated with full light from a xenon lamp, and the MB solution was collected every 0.5 h. The absorbance of the MB solution was measured after filtering through a filter head. The degradation efficiency was calculated by formula (I). Finally, the degradation of the dye was determined by ultraviolet spectrophotometry.
[0097] The results are as follows Figure 4-6 As shown. Figure 4 When 0.02-0.04g STA / 3N-TiO2 was added to the methylene blue solution, there was an obvious removal effect on methylene blue. Among them, the highest removal efficiency of methylene blue was achieved when the dosage was 0.03g after 120 minutes of illumination, and the removal rate at this time could reach 91.32%.
[0098] like Figure 5 When 0.02-0.04g STA / 2N-TiO2 was added to the methylene blue solution, there was an obvious removal effect on methylene blue. Among them, the highest removal efficiency of methylene blue was when the dosage was 0.03g after 120min of illumination, and the removal rate at this time could reach 84.47%.
[0099] like Figure 6 When 0.02-0.04g STA / 4N-TiO2 was added to the methylene blue solution, there was an obvious removal effect on methylene blue. Among them, the highest removal efficiency of methylene blue was when the dosage was 0.03g after 120min of illumination, and the removal rate at this time could reach 85.48%.
[0100] Example 8 :
[0101] In this example, the water contact angle of the N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating flat plate with different nitrogen doping amounts obtained in Examples 1-3 was measured using a surface contact angle measuring instrument.
[0102] The results are as follows Figure 5 As shown, the contact angle of the PDMS / STA / 3N-TiO2 coating prepared in Example 1 is 170.9°; and the contact angle of the PDMS / STA / 3N-TiO2 coating prepared in Example 1 after two weeks of outdoor exposure is 158.4°;
[0103] The contact angle of the PDMS / STA / 2N-TiO2 coating prepared in Example 2 is 159.7°;
[0104] The contact angle of the PDMS / STA / 4N-TiO2 coating prepared in Example 3 is 157.4°;
[0105] The contact angle of the PDMS / STA / TiO2 coating prepared in Comparative Example 1 was 153.8°;
[0106] The contact angle of the PDMS / STA / 3N-TiO2(R) coating prepared in Comparative Example 2 is 156.8°.
[0107] From the water contact angle measurement value, it can be seen that the surface water contact angle of the coating flat plate obtained by Examples 1-3 and Comparative Examples 1 and 2 is greater than 150 °, showing excellent super hydrophobic performance. However, the surface water contact angle of Examples 1-3 is greater than that of the comparative example, which may be due to the addition of nitrogen element by hydrothermal method, which changes the performance of the nano material and improves its hydrophobic ability. In addition, after two weeks of outdoor exposure test, the coating still has excellent super hydrophobic performance, proving that the coating material has good stability.
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A fluorine-free preparation method for a N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating, characterized in that: The following steps are involved: S1, adding urea to a solution of methanol, tetrabutyl titanate and acetylacetone and performing ultrasonic treatment; S2, mixing the reaction solution obtained in step S1 with anhydrous ethanol uniformly, and then performing hydrothermal reaction and centrifugal washing in sequence; S3, drying, grinding and calcining the material obtained in step S2 in sequence to obtain a loose and porous N-TiO2 material; S4, dissolving the N-TiO2 material in an organic solvent, adding stearic acid for hydrophobic modification after ultrasonic treatment, and then centrifugally washing, drying and grinding in sequence to obtain STA / N-TiO2 material; S5. Disperse STA / N-TiO2 material and polydimethylsiloxane in ethyl acetate, then apply it on a glass slide, and obtain a PDMS / STA / N-TiO2 coating after curing.
2. The preparation method according to claim 1, characterized in that In step S1, the mass ratio of methanol, tetrabutyl titanate and acetylacetone is 13:3:1 to 13:3.4:1; preferably, the mass ratio of methanol, tetrabutyl titanate and acetylacetone is 13:3.2:
1.
3. The preparation method according to claim 1, characterized in that: In step S2, the reaction temperature of the hydrothermal reaction is 180-240° C., and the reaction time is 3-6 hours; preferably, the reaction temperature of the hydrothermal reaction is 220° C., and the reaction time is 5 hours.
4. The preparation method according to claim 1, characterized in that: In step S3, the drying temperature is 80-110°C, and the drying time is 10-13 hours; preferably, the drying temperature is 100°C, and the drying time is 12 hours.
5. The preparation method according to claim 1, characterized in that: In step S3, the calcination is carried out by heating the temperature to 450-550°C at a heating rate of 1-3°C / min, and the holding time is 2.5-3.5h; preferably, the calcination is carried out by heating the temperature to 500°C at a heating rate of 2°C / min, and the holding time is 3h.
6. The preparation method according to claim 1, characterized in that: In step S4, the mass ratio of N-TiO2 and stearic acid is 1:1.1 to 1:1.3; preferably, the mass ratio of N-TiO2 and stearic acid is 1:1.
2.
7. The preparation method according to claim 1, characterized in that: In step S4, the temperature of the hydrophobic modification is 65-75°C, and the time is 2-3.5 hours; preferably, the temperature of the hydrophobic modification is 70°C, and the time is 3 hours; In step S4, the drying temperature is 75-85°C and the drying time is 6-10 hours; preferably, in step S4, the drying temperature is 80°C and the drying time is 8 hours.
8. The preparation method according to claim 1, characterized in that: In step S5, the mass ratio of STA / N-TiO2 to polydimethylsiloxane is 1:1 to 3:2; preferably, the mass ratio of STA / N-TiO2 to polydimethylsiloxane is 5:4; The curing temperature is 90-110° C., and the curing time is 22-25 hours; preferably, the curing temperature is 100° C., and the curing time is 24 hours.
9. The preparation method according to claim 1, characterized in that: In step S5, the specific method of spraying is: after the glass slide is polished, cleaned and dried, the dispersion is sprayed at a distance of about 15 cm from the glass slide.
10. A N-TiO2 photocatalytic surface self-cleaning super-hydrophobic coating material, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of nitrogen (N)-doped titanium dioxide (TiO2) microspheres
CN102513043A
Hydrophobic and ultraviolet radiation proof transparent film and preparation thereof