Immersed photoresist composition

By using polymer resin with rich functional groups and alkyl cellulose with low critical phase transition temperature in immersion photoresist, a three-dimensional network structure is formed, which solves the problems of high leaching rate and small contact angle, and improves the photoresist The stability and performance of the 193nm lithography process is suitable for 193nm lithography process.

CN119087744APending Publication Date: 2024-12-06WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411339985.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing immersion photoresist has problems with high leachate and small contact angle at 193nm wavelength, which affects the lithography performance, and the commonly used fluorine-containing additives are unstable and affects the lithography performance.

Method used

Using polymer resins with rich functional groups and alkyl cellulose with low critical phase transition temperatures, a three-dimensional network is formed through hydrogen bonds or electrostatic interactions, reducing the leachate and increasing the contact angle.

Benefits of technology

It significantly reduces the leaching rate of the photoresist, increases the contact angle, reduces the leaching of small molecules such as photoacid-induced agents, improves the stability and performance of the photoresist, and is suitable for the formation of nano-scale patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059412490000021
    Figure BDA0005059412490000021
  • Figure BDA0005059412490000022
    Figure BDA0005059412490000022
  • Figure BDA0005059412490000031
    Figure BDA0005059412490000031
Patent Text Reader

Abstract

The invention relates to an immersed photoresist composition, which is prepared from the following components in percentage by mass: 1 to 20 percent of polymer resin, 1 to 20 percent of cellulose, 0.1 to 10 percent of photoacid generator, 0.1 to 10 percent of acid diffusion inhibitor and 50 to 98 percent of organic solvent. According to the present invention, by introducing the alkyl cellulose having a polyfunctional group and a low critical phase transition temperature (LCST), the alkyl cellulose and the alkyl cellulose can form hydrogen bonds or electrostatic interaction, and the conversion from the sol to the gel can be achieved by increasing the temperature so as to form the three-dimensional network, such that the leaching rate can be effectively reduced during the 193 nm immersion lithography process, and the contact angle can be effectively increased;
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention belongs to the technical field of integrated circuits, and in particular relates to an immersion photoresist composition. Background technology:

[0002] Photoresist, also known as photoresist, is the most critical material in the photolithography process. The pattern on the mask is projected onto the photoresist, stimulating a photochemical reaction, and forming a photoresist pattern after baking and development. As the resolution continues to be higher and the feature size continues to decrease, the exposure wavelength of the photolithography machine is also required to be continuously reduced, from the initial i-line (365nm) and KrF (248nm) to the current advanced process ArF (193nm) and EUV (13.5nm). Among them, ArF lithography is divided into dry and wet methods. The so-called wet method is to fill the space between the photolithography machine lens and the photoresist with water, so it is also called immersion lithography. This puts forward some special requirements for immersion photoresist. First, the active ingredients of the photoresist cannot be leached in water, otherwise it will contaminate the photolithography machine lens; second, the photoresist must have strong hydrophobicity, otherwise the diffusion of water into the photoresist will cause the colloid to swell and the loss of photosensitivity. In order to improve the leaching rate and contact angle of immersion photoresist, the commonly used method is to add fluorine-containing additives or fluorine-containing resins with low surface energy. For example, patents CN114349898A and CN115806641A disclose a photoresist fluorine-containing resin for improving the hydrophobicity of the photoresist surface, but fluorine monomers are often difficult to obtain and are mostly unstable, and fluorine-containing additives or fluorine-containing resins will affect the photolithographic performance of the photoresist to a certain extent, limiting the development of immersion photoresists. Summary of the invention:

[0003] To solve the above problems, the present application provides a photoresist composition, which uses a polymer resin with rich functional groups and introduces an alkyl cellulose with multiple functional groups and a low critical phase transition temperature (LCST). The two can form hydrogen bonds or electrostatic interactions, and the transition from sol to gel can be achieved by increasing the temperature, thereby forming a three-dimensional network, which can effectively reduce the leaching rate and increase the contact angle during the 193nm immersion lithography process.

[0004] To achieve the purpose of the present invention, the present invention provides the following technical solutions:

[0005] An immersion photoresist composition, characterized in that it comprises the following components in mass fractions:

[0006] Polymer resin 1-20%, preferably 2-10%;

[0007] Cellulose 1-20%, preferably 2-10%;

[0008] Photoacid generator 0.1-10%, preferably 0.5-2%;

[0009] Acid diffusion inhibitor 0.1-10%, preferably 0.5-2%;

[0010] Organic solvent 50-98%, preferably 80-95%;

[0011] Preferably, the polymer resin comprises an acid-sensitive monomer structural unit and a polar monomer structural unit,

[0012] Wherein, the acid-sensitive monomer structural unit is as follows:

[0013]

[0014] Wherein, R1 is H or a carbon chain with 1-20 carbon atoms; R2 is connected to the oxygen atom and is a tertiary carbon atom, and all hydrogen atoms on this carbon atom are replaced by other groups, and its possible structure is one or more of tert-butyl, substituted tert-butyl, alkyl-substituted adamantane, alkyl-substituted adamantane derivative, alkyl-substituted norbornene, alkyl-substituted norbornene derivative, alkyl-substituted cyclic alkyl, alkyl-substituted cyclic alkyl derivative, etc.;

[0015] Preferably, R1 is H or a carbon chain with 1 to 5 carbon atoms, and R2 is an alkyl-substituted adamantane, an alkyl-substituted norbornene, or an alkyl-substituted cyclic alkyl.

[0016] More preferably, R1 is H or a carbon chain having 1 to 3 carbon atoms, and R2 is adamantane substituted with methyl, ethyl, propyl or isopropyl, or a cyclic alkyl substituted with methyl, ethyl, propyl or isopropyl.

[0017] The polar monomer structural unit is as follows:

[0018]

[0019] Wherein R3 is H or a carbon chain with 1-20 carbon atoms; R4 is a lactone structure with 6-30 carbon atoms or a cyclic, cage-like or linear carbon-containing structure containing hydroxyl groups, or preferably one or more of adamantane containing one or more independent hydroxyl groups, cyclohexyl ester containing one or more independent hydroxyl groups, cyclopentyl ester containing one or more independent hydroxyl groups, polycyclic ester compounds containing one or more independent hydroxyl groups, cage-like ester compounds containing one or more independent hydroxyl groups, butyrolactone, valerolactone, substituted valerolactone, caprolactone, substituted caprolactone, lactone containing norbornene structure, lactone containing adamantane structure, lactone containing polycyclic structure, lactone containing cage-like structure, etc.

[0020] Preferably, R3 is H or a carbon chain with 1-5 carbon atoms, and R4 is adamantane containing an independent hydroxyl group, a lactone containing a norbornene structure, a lactone containing an adamantane structure, or a lactone containing a polycyclic structure.

[0021] More preferably, R3 is H or a carbon chain with 1-3 carbon atoms, and R4 is adamantane containing one independent hydroxyl group, a lactone containing a norbornene structure, or a lactone containing a 5- to 8-membered ring structure.

[0022] Preferably, the weight average molecular weight of the polymer resin is 1000 to 100000, more preferably 5000 to 30000;

[0023] Preferably, the molar ratio of the acid-sensitive monomer structural unit to the polar monomer structural unit in the polymer resin is 2-8:8-2, preferably 4-6:5.

[0024] Preferably, the polymer resin is prepared by polymerizing an acid-sensitive monomer and a polar monomer.

[0025] The structure of the acid-sensitive monomer is:

[0026]

[0027] Wherein, R1 and R2 have the same meanings as above.

[0028] The structure of the polar monomer is:

[0029]

[0030] Wherein, R3 and R4 have the same meanings as above.

[0031] The cellulose is alkyl cellulose or hydroxy-substituted alkyl cellulose. Alkyl cellulose or hydroxy-substituted alkyl cellulose has a low critical phase transition temperature and abundant functional groups. The temperature can be raised to realize the transition from sol to gel, and hydrogen bonds or electrostatic interactions are formed with the functional groups on the resin, thereby forming a three-dimensional network structure. Preferably, the alkyl cellulose includes one or more of methyl cellulose, ethyl cellulose, and propyl cellulose, and the hydroxy-substituted alkyl cellulose includes one or more of hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, and hydroxybutyl methyl cellulose;

[0032] The photoacid generator is selected from one or more of sulfonium salts and iodonium salts, preferably perfluorobutyl triphenyl sulfonium salt, trifluoromethyl triphenyl sulfonium salt, o-trifluoromethylphenyl triphenyl sulfonium salt, p-trifluoromethylphenyl triphenyl sulfonium salt, perfluorobutyl diphenyl iodonium salt, trifluoromethyl diphenyl iodonium salt, o-trifluoromethylphenyl diphenyl iodonium salt, p-trifluoromethylphenyl diphenyl iodonium salt, bis (4-tert-butylphenyl) iodine camphor sulfonate, bis (4-tert-butylphenyl) iodine trifluoromethanesulfonate, more preferably one or more of perfluorobutyl triphenyl sulfonium salt, o-trifluoromethylphenyl triphenyl sulfonium salt and perfluorobutyl diphenyl iodonium salt.

[0033] Preferably, the acid diffusion inhibitor is an amine compound, including any one or more of trioctylamine, tetrabutylammonium hydroxide, 2-methoxyethoxyethyl-2-triamine, isopropanolamine, N,N-dimethylaminoethyl acetate, N,N-dimethylglycine, 2,6-dioxaheptylamine, 4,4'-diaminodiphenyl ether, N-tert-butoxycarbonyl dioctylamine, N,N-dimethylformamide, acetamide, N-methylacetamide and benzamide.

[0034] The organic solvent is selected from one or more of ketone solvents, polyols, alkyl ethers, alkyl ester solvents, and amide solvents, preferably acetone, methyl ethyl ketone, cyclohexanone, methyl isoamyl ketone, 2-heptanone, ethylene glycol, ethylene glycol monoacetate, diethylene glycol, ethylene glycol monoacetate, propylene glycol, propylene glycol monoacetate, dipropylene glycol and dipropylene glycol monoacetate, and their monomethyl, monoethyl, monopropyl, monobutyl and monophenyl ethers, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone One or more, more preferably 2-heptanone, propylene glycol monomethyl ether, propylene glycol methyl ether acetate one or more.

[0035] The photoresist composition of the invention is applicable to the field of 193nm immersion lithography, is suitable for forming nanometer-scale patterns in integrated circuits, and is applied to the field of chip manufacturing.

[0036] Compared with the prior art, this application has the following beneficial effects:

[0037] In the present photoresist, a resin with abundant functional groups (such as hydroxyl groups, ester groups, etc.) is used, and an alkyl cellulose with multiple functional groups and a low critical phase transition temperature (LCST) is introduced. The two can form hydrogen bonds or electrostatic interactions, and the transition from sol to gel can be achieved by increasing the temperature, forming a three-dimensional network and a protective layer, thereby reducing the leaching of small molecules such as photoacid generators and acid diffusion inhibitors out of the photoresist, and the formed protective layer can increase the contact angle of the photoresist and reduce water residue. Specific implementation method:

[0038] The specific implementation scheme of the method is further described below in conjunction with examples. However, the present invention is not limited to the listed embodiments, and should also include any other known changes within the scope of the rights claimed by the present invention.

[0039] In the various embodiments and comparative examples of the present invention, the sources of the main raw materials are as follows. Unless otherwise specified, other raw materials and reagents are purchased through common commercial channels:

[0040] Methylcellulose was purchased from Beijing Bailingwei Technology Co., Ltd.;

[0041] Ethyl cellulose was purchased from Beijing Bailingwei Technology Co., Ltd.;

[0042] Hydroxypropyl cellulose was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;

[0043] Hydroxypropyl methylcellulose was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;

[0044] Hydroxyethyl cellulose was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;

[0045] Hydroxybutyl methylcellulose was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;

[0046] 1-Isopropylcyclopentyl methacrylate was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0047] 2-Carboxyl-4-norbornyl lactone-5-methacrylate was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0048] 2-Methyl-2-methacrylate adamantane was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0049] 2-Carbonyl-tetrahydrofuran-3-hydroxy-methylacrylate was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0050] 1-Methyl-1-cyclohexyl methacrylate was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0051] 1,7,7-Trimethylbicyclo[2.2.1]hept-2-yl methacrylate was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0052] 2-Ethyl-2-adamantyl methacrylate was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0053] r-Butyrolactone-3-yl isomethacrylate was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0054] 1-Methylcyclopentyl methacrylate was purchased from China Energy Conservation Wanrun Co., Ltd.;

[0055] 3-Hydroxy-1-adamantyl methacrylate was purchased from Shanghai Huaen Yi New Material Technology Co., Ltd.

[0056] Preparation of polymer resin Polymer-A: 30g of propylene glycol monomethyl ether acetate (PGMEA) was placed in a three-necked flask, replaced with nitrogen, and heated to 80°C. Monomer 1-isopropylcyclopentyl methacrylate (19.63g), 2-carboxy-4-norbornyl lactone-5-methacrylate (22.22g), and initiator azobisisobutyronitrile (0.88g) were dissolved in 60g of PGMEA. The above solution was added dropwise to the three-necked flask within 3 hours and kept warm for 2 hours. After the reaction was completed, the reactants were cooled to room temperature. Precipitation was carried out in 1.5 kg of methyl tert-butyl ether (MTBE), the precipitated polymer was collected by filtration, air-dried overnight, redissolved in 120 g of tetrahydrofuran, and then precipitated into 1.6 kg of MTBE. The final polymer was filtered, air-dried overnight, and then vacuum-dried at 60° C. for 48 h to obtain polymer resin Polymer-A (Mw=9680, PDI=1.58).

[0057] Preparation of polymer resin Polymer-B: 30g of propylene glycol monomethyl ether acetate (PGMEA) was placed in a three-necked flask, replaced with nitrogen, and heated to 80°C. The monomer 2-methyl-2-methyl methacrylate adamantyl ester (23.43g), 2-carbonyl-tetrahydrofuran-3-hydroxy-methylacrylate (17.02g), and initiator azobisisobutyronitrile (0.88g) were dissolved in 60g of PGMEA. The above solution was added dropwise to the three-necked flask within 3 hours and kept warm for 2 hours. After the reaction was completed, the reactants were cooled to room temperature. Precipitation was carried out in 1.5 kg of methyl tert-butyl ether (MTBE), the precipitated polymer was collected by filtration, air-dried overnight, redissolved in 120 g of tetrahydrofuran, and then precipitated into 1.6 kg of MTBE. The final polymer was filtered, air-dried overnight, and then vacuum-dried at 60° C. for 48 h to obtain polymer resin Polymer-B (Mw=13350, PDI=1.62).

[0058] Preparation of polymer resin Polymer-C: 30g of propylene glycol monomethyl ether acetate (PGMEA) was placed in a three-necked flask, replaced with nitrogen, and heated to 80°C. The monomer 1-methyl-1-cyclohexyl methacrylate (18.23g), 1,7,7-trimethylbicyclo[2.2.1]hept-2-yl methacrylate (22.23g), and initiator azobisisobutyronitrile (0.88g) were dissolved in 60g of PGMEA. The above solution was added dropwise to the three-necked flask within 3 hours and kept warm for 2 hours. After the reaction was completed, the reactants were cooled to room temperature. Precipitation was carried out in 1.5 kg of methyl tert-butyl ether (MTBE), the precipitated polymer was collected by filtration, air-dried overnight, redissolved in 120 g of tetrahydrofuran, and then precipitated into 1.6 kg of MTBE. The final polymer was filtered, air-dried overnight, and then vacuum-dried at 60° C. for 48 h to obtain polymer resin Polymer-C (Mw=10065, PDI=1.54).

[0059] Preparation of polymer resin Polymer-D: 30g of propylene glycol monomethyl ether acetate (PGMEA) was placed in a three-necked flask, replaced with nitrogen, and heated to 80°C. The monomer 2-ethyl-2-adamantyl methacrylate (24.84g), r-butyrolactone-3-yl isomethacrylate (17.02g), and initiator azobisisobutyronitrile (0.88g) were dissolved in 60g of PGMEA. The above solution was added dropwise to the three-necked flask within 3 hours and kept warm for 2 hours. After the reaction was completed, the reactants were cooled to room temperature. The precipitated polymer was collected by filtration, air-dried overnight, redissolved in 120 g of tetrahydrofuran, and precipitated into 1.6 kg of MTBE. The final polymer was filtered, air-dried overnight, and then vacuum-dried at 60° C. for 48 h to obtain a polymer resin Polymer-D (Mw=9975, PDI=1.57).

[0060] Preparation of polymer resin Polymer-E: 30g of propylene glycol monomethyl ether acetate (PGMEA) was placed in a three-necked flask, replaced with nitrogen, and heated to 80°C. The monomer 1-methylcyclopentyl methacrylate (16.82g), 3-hydroxy-1-adamantyl methacrylate (23.63g), and initiator azobisisobutyronitrile (0.88g) were dissolved in 60g of PGMEA. The above solution was added dropwise to the three-necked flask within 3 hours and kept warm for 2 hours. After the reaction was completed, the reactants were cooled to room temperature. Precipitation was carried out in 1.5kg of methyl tert-butyl ether (MTBE), the precipitated polymer was filtered and collected, air-dried overnight, dissolved in 120g of tetrahydrofuran, and precipitated in 1.6kg of MTBE. The final polymer was filtered, air-dried overnight, and then vacuum-dried at 60°C for 48h to obtain polymer resin Polymer-E (Mw=11230, PDI=1.65).

[0061] Preparation of photoresist: Table 1 shows the photoresist formulations of the embodiments and comparative examples. The resin, photoacid generator, acid diffusion inhibitor, and alkyl cellulose were dissolved in an organic solvent for 6 hours and then filtered through a filter with a pore size of 0.1 um to obtain a photoresist composition.

[0062] Table 1 Photoresist formula

[0063]

[0064]

[0065] Test example:

[0066] A total of 9 photoresists of Examples 1 to 6 and Comparative Examples 1 to 3 were used to spin-coat the photoresists on silicon wafers treated with hexamethyldisilazane. The rotation speed was adjusted so that the film thickness after drying was about 100 nm. The drying process was to bake the silicon wafer coated with the photoresist on a 90°C hot plate for 90 seconds. The instrument used in the whole process was TEL Track act 8. Finally, a photoresist film was obtained.

[0067] Leaching test: The photoresist film was exposed to flowing deionized water for different time periods, and the chemical composition in the water sample was measured as a function of the photoresist contact time to obtain the leaching rate. The results are shown in Table 2.

[0068] Table 2 Leaching test results

[0069] <![CDATA[Leaching rate / (×10 -12 mol / cm 2 / s)]]> Example 1 0.04 Example 2 0.07 Example 3 0.03 Example 4 0.05 Example 5 0.03 Example 6 0.07 Comparative Example 1 0.78 Comparative Example 2 1.12 Comparative Example 3 0.95

[0070] Contact angle test: At room temperature, deionized water was used as the liquid, and the droplet size was 0.2 to 2 μl. The static contact angle of the photoresist film to water was tested. The above-mentioned photoresist films were tested separately, and each sample was tested 5 times in parallel. The average values ​​were shown in Table 3 below.

[0071] Table 3 Contact angle test results

[0072] Contact angle / ° Example 1 98.21 Example 2 99.83 Example 3 103.74 Example 4 101.24 Example 5 102.13 Example 6 102.94 Comparative Example 1 81.57 Comparative Example 2 85.78 Comparative Example 3 83.26

[0073] From the comparison of the test results, it can be seen that the introduction of alkyl cellulose with multiple functional groups and low critical phase transition temperature into the photoresist can reduce the leaching rate of the photoresist by one order of magnitude through interaction with the resin, and increase the contact angle by more than 10°. It can significantly reduce the contamination of the lens by small molecules such as photoacid generators during 193nm immersion photoresist exposure, reduce the generation of defects in the manufacturing process, and has good application prospects.

[0074] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. An immersion photoresist composition, characterized in that The following components are included in the mass fraction: Polymer resin 1-20%, preferably 2-10%; Cellulose 1-20%, preferably 2-10%; Photoacid generator 0.1-10%, preferably 0.5-2%; Acid diffusion inhibitor 0.1-10%, preferably 0.5-2%; The organic solvent is 50-98%, preferably 80-95%.

2. The composition according to claim 1, characterized in that The polymer resin includes an acid-sensitive monomer structural unit and a polar monomer structural unit. Wherein, the acid-sensitive monomer structural unit is as follows: Wherein, R1 is H or a carbon chain with 1-20 carbon atoms; R2 is connected to the oxygen atom and is a tertiary carbon atom, and all hydrogen atoms on this carbon atom are replaced by other groups, and its possible structure is one or more of tert-butyl, substituted tert-butyl, alkyl-substituted adamantane, alkyl-substituted adamantane derivative, alkyl-substituted norbornene, alkyl-substituted norbornene derivative, alkyl-substituted cyclic alkyl, and alkyl-substituted cyclic alkyl derivative; Preferably, R1 is H or a carbon chain with 1 to 5 carbon atoms, and R2 is an alkyl-substituted adamantane, an alkyl-substituted norbornene, or an alkyl-substituted cyclic alkyl; More preferably, R1 is H or a carbon chain having 1 to 3 carbon atoms, and R2 is a methyl, ethyl, propyl or isopropyl substituted adamantane, a methyl, ethyl, propyl or isopropyl substituted cyclic alkyl; The polar monomer structural unit is as follows: Wherein R3 is H or a carbon chain with 1-20 carbon atoms; R4 is a lactone structure with 6-30 carbon atoms or a cyclic, cage-like or linear carbon-containing structure containing hydroxyl groups, or preferably one or more of adamantane containing one or more independent hydroxyl groups, cyclohexyl ester containing one or more independent hydroxyl groups, cyclopentyl ester containing one or more independent hydroxyl groups, polycyclic ester compounds containing one or more independent hydroxyl groups, cage-like ester compounds containing one or more independent hydroxyl groups, butyrolactone, valerolactone, substituted valerolactone, caprolactone, substituted caprolactone, lactone containing norbornene structure, lactone containing adamantane structure, lactone containing polycyclic structure, and lactone containing cage-like structure; Preferably, R3 is H or a carbon chain with 1-5 carbon atoms, and R4 is adamantane containing an independent hydroxyl group, a lactone containing a norbornane structure, a lactone containing an adamantane structure, or a lactone containing a polycyclic structure; More preferably, R3 is H or a carbon chain with 1-3 carbon atoms, and R4 is adamantane containing one independent hydroxyl group, a lactone containing a norbornene structure, or a lactone containing a 5- to 8-membered ring structure.

3. The composition according to claim 1 or 2, characterized in that The weight average molecular weight of the polymer resin is 1,000 to 100,000, more preferably 5,000 to 30,000.

4. The composition according to any one of claims 1 to 3, characterized in that The molar ratio of the acid-sensitive monomer structural unit to the polar monomer structural unit in the polymer resin is 2-8:8-2, preferably 4-6:

5.

5. The composition according to any one of claims 1 to 4, characterized in that The polymer resin is prepared by polymerizing an acid-sensitive monomer and a polar monomer.

6. The composition according to any one of claims 1 to 5, characterized in that The structure of the acid-sensitive monomer is: Wherein, R1 and R2 have the same meaning as in claim 2; The structure of the polar monomer is: Wherein, R3 and R4 have the same meaning as in claim 2.

7. The composition according to any one of claims 1 to 6, characterized in that The cellulose is alkyl cellulose or hydroxy-substituted alkyl cellulose; preferably, the alkyl cellulose includes one or more of methyl cellulose, ethyl cellulose, and propyl cellulose, and the hydroxy-substituted alkyl cellulose includes one or more of hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, and hydroxybutyl methyl cellulose.

8. The composition according to any one of claims 1 to 7, characterized in that The photoacid generator is selected from one or more of sulfonium salts and iodonium salts, preferably perfluorobutyl triphenyl sulfonium salt, trifluoromethyl triphenyl sulfonium salt, o-trifluoromethylphenyl triphenyl sulfonium salt, p-trifluoromethylphenyl triphenyl sulfonium salt, perfluorobutyl diphenyl iodonium salt, trifluoromethyl diphenyl iodonium salt, o-trifluoromethylphenyl diphenyl iodonium salt, p-trifluoromethylphenyl diphenyl iodonium salt, bis (4-tert-butylphenyl) iodine camphor sulfonate, bis (4-tert-butylphenyl) iodine trifluoromethanesulfonate, more preferably one or more of perfluorobutyl triphenyl sulfonium salt, o-trifluoromethylphenyl triphenyl sulfonium salt and perfluorobutyl diphenyl iodonium salt.

9. The composition according to any one of claims 1 to 8, characterized in that The acid diffusion inhibitor is an amine compound, including any one or more of trioctylamine, tetrabutylammonium hydroxide, 2-methoxyethoxyethyl-2-triamine, isopropanolamine, N,N-dimethylaminoethyl acetate, N,N-dimethylglycine, 2,6-dioxaheptylamine, 4,4'-diaminodiphenyl ether, N-tert-butoxycarbonyl dioctylamine, N,N-dimethylformamide, acetamide, N-methylacetamide and benzamide.

10. The composition according to any one of claims 1 to 9, characterized in that The organic solvent is selected from one or more of ketone solvents, polyols, alkyl ethers, alkyl ester solvents, and amide solvents, preferably acetone, methyl ethyl ketone, cyclohexanone, methyl isoamyl ketone, 2-heptanone, ethylene glycol, ethylene glycol monoacetate, diethylene glycol, ethylene glycol monoacetate, propylene glycol, propylene glycol monoacetate, dipropylene glycol and dipropylene glycol monoacetate, and their monomethyl, monoethyl, monopropyl, monobutyl and monophenyl ethers, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone One or more, more preferably 2-heptanone, propylene glycol monomethyl ether, propylene glycol methyl ether acetate one or more.