Single-component epoxy sealant as well as preparation method and application thereof
By using single-component epoxy sealant in wearable smart electronic products, the problems of complex operation, poor waterproof performance and poor sealing performance are solved, and the effects of high bond strength and low shrinkage are achieved, satisfying the multifunctional and High performance requirements for miniaturization development.
Patent Information
- Application Number
- CN202411154631.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing sealant has problems such as complex operation, poor waterproofing performance, poor sealing performance, large shrinkage and low bonding strength in wearable smart electronic products, and cannot meet the high-performance requirements of multifunctionalization and miniaturization development.
Provide a single component epoxy sealant, including solid epoxy resin, low viscosity epoxy resin, rubber modified epoxy resin, cashew phenol epoxy active diluent, acid anhydride mixture and modified imidazole, by specific synthetic methods and component ratio to improve its flexibility, sealing and bonding strength.
It achieves easy operation of single-component, good waterproof performance, good sealing performance, low shrinkage and high bonding strength, meeting the sealing and protection needs of wearable smart electronic products.
Smart Images

Figure BDA0005004591370000031 
Figure BDA0005004591370000041 
Figure BDA0005004591370000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adhesives, and in particular to a one-component epoxy sealant and a preparation method and application thereof. Background Art
[0002] As an emerging technology, wearable smart electronic products are widely used in the fields of life health, medical care, sports, etc., mainly through various sensors and software technologies to monitor human physiological functions. Wearable smart electronic products are developing in the direction of multi-functionality and miniaturization, and the micro-assembly technology of various key components is also developing rapidly. At the same time, sensor technology is also developing towards new technical trends such as high precision, multi-dimensionality, and virtual multi-functionality. Sealant seals and protects wearable smart electronic products and related sensor components, making the process operability of wearable smart electronic products good and the bonding strength high, effectively improving the functionality, practicality and reliability of wearable smart electronic products.
[0003] Currently, most of the sealants available on the market have problems such as complex operation, poor waterproof performance, poor sealing performance, large shrinkage, and low bonding strength. They cannot meet the various high-performance requirements brought about by the development of wearable product technology towards multifunctionality and miniaturization. Summary of the invention
[0004] In order to solve the above technical problems existing in the prior art, the present invention provides a one-component epoxy sealant and a preparation method thereof.
[0005] The technical solution of the present invention to solve the above technical problems is as follows:
[0006] The first aspect of the present invention is to provide a one-component epoxy sealant, which comprises the following components by weight:
[0007] 10-20 parts of solid epoxy resin, 20-35 parts of low viscosity epoxy resin, 10-15 parts of rubber modified epoxy resin, 10-13 parts of cardanol epoxy reactive diluent, 32-35 parts of acid anhydride mixture, and 3-5 parts of modified imidazole.
[0008] On the basis of the above technical solution, the present invention can also make the following technical improvements:
[0009] Furthermore, the solid epoxy resin has a molecular weight of 1345 to 1395, an epoxy equivalent of 800 to 835 g / eq, and a softening point of 87 to 95°C.
[0010] Furthermore, the solid epoxy resin is prepared by the following method: according to the mass fractions, 71 to 72 parts of epoxy resin and 28 to 29 parts of diphenol propane are added into a reaction kettle, heated to 140 to 160° C., set the speed to 10 RPM, and stirred for 1 to 2 hours until completely dissolved; cooled to 95 to 105° C., maintained at a speed of 10 RPM, and added 0.05 to 0.1 parts of a catalyst; then heated to 185 to 195° C., vacuumed, set the speed to 30 RPM, and stirred for 2 to 3 hours to obtain the solid epoxy resin.
[0011] Furthermore, the epoxy resin is a bisphenol A epoxy resin with a molecular weight of 338-346 and an epoxy equivalent of 188-198 g / eq; the diphenol propane has a molecular weight of 216-228 and a melting point of 158-159° C.; and the catalyst is ethyl triphenyl phosphonium bromide with a molecular weight of 265-371 and a melting point of 204-207° C.
[0012] The beneficial effects of adopting the above further technical scheme are: the synthesis mechanism of the solid epoxy resin is that the oxygen atom of the epoxy group in the epoxy resin undergoes a Michael addition reaction with the hydroxyl group in the diphenol propane under the catalytic action of ethyl triphenyl phosphonium bromide; the solid epoxy resin has a large molecular weight, which can increase the flexibility and sealing of the system, and at the same time has good waterproof performance; the molecular chain grafted benzene ring hybrid structure has excellent thermal stability and low shrinkage performance.
[0013] Furthermore, the epoxy resin is HBEL-123 produced by Dongying Hebang Chemical Co., Ltd.
[0014] The beneficial effect of adopting the above further technical solution is that the epoxy resin HBEL-123 has excellent reactivity and bonding strength, which is conducive to further improving the bonding strength and sealing performance of the solid epoxy resin.
[0015] Furthermore, the diphenol propane is diphenol propane produced by Huangshan Shanfu Chemical Co., Ltd.
[0016] Furthermore, the catalyst is ethyl triphenylphosphonium bromide produced by Shanghai Yuanye Biotechnology Co., Ltd., which has the structural formula shown in Formula I:
[0017]
[0018] The beneficial effect of adopting the above further technical solution is that the ethyltriphenylphosphonium bromide shows high catalytic efficiency, steadily accelerates the reaction rate, and the product has good heat resistance and flexibility compared with other phosphorus-based catalysts and imidazole catalysts.
[0019] Furthermore, the low-viscosity epoxy resin is a bisphenol F-type epoxy resin with a viscosity of 800 to 1500 mPa·s at 25°C and an epoxy equivalent of 155 to 165 g / eq; the rubber-modified epoxy resin is a nano-core-shell rubber-modified epoxy resin with a viscosity of 6000 to 9000 mPa·s at 50°C and an epoxy equivalent of 260 to 275 g / eq; the cardanol epoxy reactive diluent is a cardanol-modified epoxy reactive diluent with a viscosity of 90 to 200 mPa·s at 25°C and an epoxy equivalent of 250 to 300 g / eq; the modified imidazole is an imidazole adduct with an average particle size of 2-4 μm and a reaction temperature of 100°C.
[0020] Furthermore, the low-viscosity epoxy resin is HBEL-153 produced by Dongying Hebang Chemical Co., Ltd.
[0021] The beneficial effect of adopting the above further technical solution is that the low-viscosity epoxy resin has the characteristics of low viscosity, high bonding strength and low shrinkage.
[0022] Furthermore, the rubber-modified epoxy resin is MX267 produced by Kaneka Corporation of Japan.
[0023] The beneficial effect of adopting the above further technical solution is that the rubber modified epoxy resin is a nano core-shell rubber modified epoxy resin toughening agent, the nano core-shell rubber is uniformly dispersed in the epoxy resin, and has excellent strength and toughness, heat resistance and impact resistance.
[0024] Further, the cardanol epoxy reactive diluent is LITE513DF produced by Cardolite Chemical Co., Ltd. of the United States, which has the structural formula shown in Formula II:
[0025]
[0026] The beneficial effect of adopting the above further technical solution is that the cardanol epoxy reactive diluent has a long aliphatic side chain, exhibits strong hydrophobicity, good water resistance and good flexibility.
[0027] Furthermore, the imidazole adduct is PN-23J produced by Ajinomoto Co., Ltd. of Japan.
[0028] The beneficial effect of adopting the above further scheme is that the imidazole adduct can accelerate the reaction rate of the acid anhydride mixture and the epoxy resin, and the product has the characteristics of low shrinkage, good heat resistance and good water resistance.
[0029] Furthermore, the acid anhydride mixture is prepared by the following method: 18 to 20 parts by mass of dodecenyl succinic anhydride, 79 to 80 parts by mass of methyl hexahydrophthalic anhydride, and 1 to 3 parts by mass of propylene glycol are sequentially put into a stirring kettle, the speed is set to 10 RPM under nitrogen protection conditions, and the mixture is stirred for 0.5 to 1 hour to obtain the acid anhydride mixture.
[0030] The beneficial effects of adopting the above further technical solution are: the obtained acid anhydride mixture has a longer terminal molecular chain, which can increase the flexibility and sealing of the system, and at the same time has good water resistance and adhesion properties; propylene glycol, as a molecular chain transfer agent, has good control reaction performance and reduces the volume shrinkage effect of the system caused by molecular cross-linking.
[0031] Furthermore, the dodecenylsuccinic anhydride is an aliphatic anhydride with a molecular weight of 262-270 and an acid value of 395-425 mgKOH / g; the methylhexahydrophthalic anhydride is an anhydride compound with a molecular weight of 164-172 and an acid value of 640-650 mgKOH / g.
[0032] Furthermore, the dodecenyl succinic anhydride is CA-I-05 produced by Guangdong Huajinda New Materials Co., Ltd.
[0033] Furthermore, the methylhexahydrophthalic anhydride is HNA-100 produced by Hitachi, Ltd. of Japan.
[0034] Furthermore, the glycerol is glycerol produced by Henan Changyuan Chemical Products Co., Ltd.
[0035] The second aspect of the present invention is to provide a method for preparing the above-mentioned one-component epoxy sealant, comprising the following steps: according to the mass fractions, solid epoxy resin, low viscosity epoxy resin, rubber modified epoxy resin, cardanol epoxy reactive diluent, acid anhydride mixture, and modified imidazole are sequentially put into a stirring kettle, vacuuming, setting the speed to 30RPM, stirring for 3 to 4 hours, and obtaining the one-component epoxy sealant.
[0036] Another aspect of the present invention is to provide application of the above-mentioned one-component epoxy sealant in wearable smart electronic products.
[0037] Compared with the prior art, the present invention has the following technical effects:
[0038] The one-component epoxy sealant of the present invention has the characteristics of single-component and easy operation, which effectively meets the process diversity of wearable intelligent electronic products; it has good waterproof performance, good sealing performance, and low shrinkage performance, which effectively guarantees the sealing protection requirements of sensors in wearable intelligent electronic products; it has high bonding strength, is suitable for the sealing bonding of various wearable intelligent electronic product shells and associated difficult-to-bond materials, and has good applicability. DETAILED DESCRIPTION
[0039] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0040] Example 1
[0041] a. By mass: 710 g of epoxy resin HBEL-123 and 290 g of diphenol propane were added to a reaction kettle, heated to 140 ° C, set the speed to 10 RPM, and stirred for 1.5 hours until completely dissolved; cooled to 95 ° C, 1 g of ethyl triphenyl phosphonium bromide was added under the stirring condition (speed 10 RPM); then heated to 185 ° C, evacuated, set the speed to 30 RPM, stirred for 3 hours to obtain a solid epoxy resin;
[0042] b. By mass: dodecenyl succinic anhydride CA-I-05 190 g, methyl hexahydrophthalic anhydride HNA-100 790 g, glycerol 20 g, successively put into a stirred tank, set the speed to 10 RPM under nitrogen protection, stirred for 1 hour to obtain an anhydride mixture;
[0043] c. By mass: 100 g of solid epoxy resin, 350 g of low viscosity epoxy resin HBEL-153, 100 g of rubber modified epoxy resin MX267, 100 g of cardanol epoxy reactive diluent LITE513DF 100 g, 350 g of anhydride mixture, and 50 g of modified imidazole PN-23J were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 3 hours to obtain a sealant.
[0044] Example 2
[0045] a. By mass: 720 g of epoxy resin HBEL-123 and 280 g of diphenol propane were added to a reaction kettle, heated to 150 ° C, set the speed to 10 RPM, and stirred for 1 hour until completely dissolved; cooled to 100 ° C, 0.5 g of ethyl triphenyl phosphonium bromide was added under the stirring condition; heated to 190 ° C, set the speed to 30 RPM under vacuum conditions, stirred for 2 hours to obtain a solid epoxy resin;
[0046] b. By mass: dodecenyl succinic anhydride CA-I-05 200g, methyl hexahydrophthalic anhydride HNA-100 800g, glycerol 10g, successively put into a stirred tank, set the speed to 10RPM under nitrogen protection, and stir for 0.5 hours to obtain an anhydride mixture;
[0047] c. By mass: 150g of solid epoxy resin, 200g of low viscosity epoxy resin HBEL-153, 150g of rubber modified epoxy resin MX267, 130g of cardanol epoxy reactive diluent LITE513DF, 330g of anhydride mixture, and 40g of modified imidazole PN-23J were sequentially put into a stirring tank, the speed was set to 30RPM under vacuum conditions, and stirred for 3 hours to obtain a sealant.
[0048] Example 3
[0049] a. By mass: 710 g of epoxy resin HBEL-123 and 290 g of diphenol propane were added to a reaction kettle, heated to 160 ° C, set the speed to 10 RPM, and stirred for 2 hours until completely dissolved; cooled to 105 ° C, 1 g of ethyl triphenyl phosphonium bromide was added under the stirring condition (speed 10 RPM); heated to 195 ° C, set the speed to 30 RPM under vacuum conditions, and stirred for 3 hours to obtain a solid epoxy resin;
[0050] b. By mass: dodecenyl succinic anhydride CA-I-05 180 g, methyl hexahydrophthalic anhydride HNA-100 790 g, glycerol 30 g, successively put into a stirred tank, set the speed to 10 RPM under nitrogen protection, and stir for 1 hour to obtain an anhydride mixture;
[0051] c. By mass: 200 g of solid epoxy resin, 250 g of low viscosity epoxy resin HBEL-153, 100 g of rubber modified epoxy resin MX267, 100 g of cardanol epoxy reactive diluent LITE513DF 100 g, 320 g of anhydride mixture, and 30 g of modified imidazole PN-23J were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 4 hours to obtain a sealant.
[0052] Comparative Example 1
[0053] a. By mass: dodecenyl succinic anhydride CA-I-05 180 g, methyl hexahydrophthalic anhydride HNA-100 790 g, glycerol 30 g, successively put into a stirred tank, set the speed to 10 RPM under nitrogen protection, and stirred for 1 hour to obtain an anhydride mixture;
[0054] c. By mass: epoxy resin HBEL-123 160g, low viscosity epoxy resin HBEL-153250g, rubber modified epoxy resin MX267 100g, cardanol epoxy reactive diluent LITE513DF 100g, anhydride mixture 360g, modified imidazole PN-23J 30g, sequentially put into a stirring tank, set the speed to 30RPM under vacuum conditions, stir for 3 hours to obtain a sealant.
[0055] Comparative Example 2
[0056] a. By mass: 710 g of epoxy resin HBEL-123 and 290 g of diphenol propane were added to a reaction kettle, heated to 160 ° C, set the speed to 10 RPM, and stirred for 2 hours until completely dissolved; cooled to 95 ° C, 1 g of ethyl triphenyl phosphonium bromide was added under the stirring condition; heated to 195 ° C, set the speed to 30 RPM under vacuum conditions, and stirred for 3 hours to obtain a solid epoxy resin;
[0057] b. By mass: dodecenyl succinic anhydride CA-I-05 180 g, methyl hexahydrophthalic anhydride HNA-100 790 g, glycerol 30 g, successively put into a stirred tank, set the speed to 10 RPM under nitrogen protection, and stir for 1 hour to obtain an anhydride mixture;
[0058] c. By mass: 200 g of solid epoxy resin, 250 g of low viscosity epoxy resin HBEL-153, 100 g of rubber-modified epoxy resin MX267, 100 g of carbon 12-14 alkyl glycidyl ether (748), 320 g of anhydride mixture, and 30 g of modified imidazole PN-23J were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 4 hours to obtain a sealant.
[0059] Comparative Example 3
[0060] a. By mass: 710 g of epoxy resin HBEL-123 and 290 g of diphenol propane were added to a reaction kettle, heated to 140 ° C, set the speed to 10 RPM, and stirred for 2 hours until completely dissolved; cooled to 105 ° C, 1 g of ethyl triphenyl phosphonium bromide was added under the stirring condition; heated to 190 ° C, set the speed to 30 RPM under vacuum conditions, and stirred for 3 hours to obtain a solid epoxy resin;
[0061] b. By mass: 200 g of solid epoxy resin, 270 g of low viscosity epoxy resin HBEL-153, 100 g of rubber modified epoxy resin MX267, 100 g of cardanol epoxy reactive diluent LITE513DF 100 g, 300 g of methyl hexahydrophthalic anhydride HNA-100, and 30 g of modified imidazole PN-23J were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 4 hours to obtain a sealant.
[0062] Comparative Example 4
[0063] a. By mass: 710 g of epoxy resin HBEL-123 and 290 g of diphenol propane were added to a reaction kettle, heated to 140 ° C, set the speed to 10 RPM, and stirred for 2 hours until completely dissolved; cooled to 105 ° C, 1 g of ethyl triphenyl phosphonium bromide was added under the stirring condition; heated to 195 ° C, set the speed to 30 RPM under vacuum conditions, and stirred for 3 hours to obtain a solid epoxy resin;
[0064] b. By mass: dodecenyl succinic anhydride CA-I-05 200g, methyl hexahydrophthalic anhydride HNA-100 800g, successively put into a stirred tank, set the speed to 10RPM under nitrogen protection, and stir for 1 hour to obtain an anhydride mixture;
[0065] c. By mass: 200 g of solid epoxy resin, 250 g of low viscosity epoxy resin HBEL-153, 100 g of rubber modified epoxy resin MX267, 100 g of cardanol epoxy reactive diluent LITE513DF 100 g, 320 g of anhydride mixture, and 30 g of modified imidazole PN-23J were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 3 hours to obtain a sealant.
[0066] The following properties of the sealants prepared in Examples 1-3 and Comparative Examples 1-4 were tested:
[0067] (1) Waterproof performance
[0068] Use an analytical balance and follow the test method for water absorption of plastics in GB / T 1034-2008: place a 61mm*61mm*1mm sample in 25℃ water for 24 hours, take it out, dry it, weigh it, and calculate the water absorption in %.
[0069] (2) Sealing performance
[0070] Use a leak tester, follow the GB / T 4208-2017 enclosure protection grade test method, 5 atmospheres, test time 1 hour, and observe whether the waterproof display label inside the sample changes color.
[0071] (3) Shrinkage performance
[0072] Use a density cup to test the liquid density of the sealant, and a density balance to test the solid density of the rubber block. Refer to GB / T39818-2021 Test method for shrinkage of thermosetting molding materials to calculate the volume shrinkage rate in %.
[0073] (4) Adhesive strength performance
[0074] Aluminum and aluminum materials were bonded with sealant. According to the GB / T 1742-1979 adhesive bond strength test method, a universal testing machine was used at a temperature of 25°C and a shear rate of 10 mm / min to test the shear strength in megapascals (MPa).
[0075] The waterproof performance is characterized by the water absorption rate, and the smaller the value, the better the waterproof performance; the sealing performance is characterized by the color change of the display label, and no color change indicates good sealing performance; the shrinkage performance is characterized by the volume shrinkage rate after curing, and the smaller the value, the smaller the shrinkage; the bonding strength is characterized by the shear strength, and the larger the value, the better the bonding strength.
[0076] The test results are shown in Table 1.
[0077] Table 1 Performance test results of various embodiments and comparative examples
[0078]
[0079] It can be seen from the data in Table 1 that the combined use of solid epoxy resin and cardanol epoxy reactive diluent has a significant benefit effect on waterproof and sealing performance, which is better than the use of either alone; the acid anhydride mixture has a significant benefit effect on shrinkage performance and bonding performance, and propylene glycol has a benefit effect on low shrinkage performance; the sealant prepared by the present invention has the advantages of single-component easy operation, good waterproof performance, good sealing performance, low shrinkage, high bonding strength, etc., and is suitable for waterproof and moisture-proof sealing and bonding of various wearable smart electronic products.
[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A one-component epoxy sealant, characterized in that: The invention comprises the following components by weight: 10 to 20 parts of solid epoxy resin, 20 to 35 parts of low-viscosity epoxy resin, 10 to 15 parts of rubber-modified epoxy resin, 10 to 13 parts of cardanol epoxy reactive diluent, 32 to 35 parts of acid anhydride mixture and 3 to 5 parts of modified imidazole.
2. The one-component epoxy sealant according to claim 1, characterized in that: The solid epoxy resin has a molecular weight of 1345 to 1395, an epoxy equivalent of 800 to 835 g / eq, and a softening point of 87 to 95°C.
3. The one-component epoxy sealant according to claim 1 or 2, characterized in that: The solid epoxy resin is prepared by the following method: according to the mass fractions, 71-72 parts of epoxy resin and 28-29 parts of diphenol propane are added into a reaction kettle, heated to 140-160° C., set the rotation speed to 10RPM, and stirred for 1-2 hours until completely dissolved; cooled to 95-105° C., maintained at a rotation speed of 10RPM, and added 0.05-0.1 parts of a catalyst; heated to 185-195° C., vacuumed, set the rotation speed to 30RPM, and stirred for 2-3 hours to obtain the solid epoxy resin.
4. The one-component epoxy sealant according to claim 3, characterized in that: The epoxy resin is a bisphenol A epoxy resin with a molecular weight of 338-346 and an epoxy equivalent of 188-198 g / eq; the diphenol propane has a molecular weight of 216-228 and a melting point of 158-159° C.; and the catalyst is ethyl triphenyl phosphonium bromide with a molecular weight of 265-371 and a melting point of 204-207° C.
5. The one-component epoxy sealant according to claim 1, characterized in that: The low-viscosity epoxy resin is a bisphenol F-type epoxy resin with a viscosity of 800-1500 mPa·s at 25°C and an epoxy equivalent of 155-165 g / eq; the rubber-modified epoxy resin is a nano-core-shell rubber-modified epoxy resin with a viscosity of 6000-9000 mPa·s at 50°C and an epoxy equivalent of 260-275 g / eq; the cardanol epoxy reactive diluent is a cardanol-modified epoxy reactive diluent with a viscosity of 90-200 mPa·s at 25°C and an epoxy equivalent of 250-300 g / eq; the modified imidazole is an imidazole adduct with an average particle size of 2-4 μm and a reaction temperature of 100°C.
6. The one-component epoxy sealant according to claim 1, characterized in that: The acid anhydride mixture is prepared by the following method: 18 to 20 parts by mass of dodecenyl succinic anhydride, 79 to 80 parts by mass of methyl hexahydrophthalic anhydride, and 1 to 3 parts of propylene glycol are sequentially added into a stirring kettle, the speed is set to 10 RPM under nitrogen protection, and the mixture is stirred for 0.5 to 1 hour to obtain the acid anhydride mixture.
7. The one-component epoxy sealant according to claim 6, characterized in that: The dodecenyl succinic anhydride is an aliphatic anhydride with a molecular weight of 262-270 and an acid value of 395-425 mgKOH / g; the methyl hexahydrophthalic anhydride is an anhydride compound with a molecular weight of 164-172 and an acid value of 640-650 mgKOH / g.
8. A method for preparing the one-component epoxy sealant according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: according to the mass fractions, solid epoxy resin, low viscosity epoxy resin, rubber modified epoxy resin, cardanol epoxy active diluent, acid anhydride mixture and modified imidazole are sequentially put into a stirring kettle, vacuuming, setting the rotation speed to 30RPM, stirring for 3 to 4 hours, and obtaining the one-component epoxy sealant.
9. Use of the one-component epoxy sealant according to any one of claims 1 to 7 in wearable smart electronic products.
Citation Information
Patent Citations
Toughened modified epoxy anhydride impregnated resin, preparation method, and application thereof
CN106750341A
Method for preparing epoxy reactive diluent
KR1020150088612A