Copolyester hot melt adhesive and preparation method thereof

By using grafting reaction of 3-methyladipic acid and vinyltriethoxysilane in copolyester hot melt adhesive and modifying nano powders with silane coupling agent, the problem of uneven material dispersion is solved and improved The elastic recovery and bonding properties of hot melt adhesives are suitable for industrial applications.

CN118931453AInactive Publication Date: 2024-11-12ZHEJIANG AOYU NEW MATERIAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411412647.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing copolyester hot melt adhesives are unevenly dispersed during the mixing process, which affects product performance and is difficult to meet the requirements of good elasticity and adhesion at the same time.

Method used

The graft reaction is carried out with 3-methyladipic acid and vinyltriethoxysilane under the action of a radical initiator to form modified 3-methyladipic acid, and the nano powder is modified by a silane coupling agent. Increase Si-O bonds and C-C bonds to improve bond strength and flexibility, and improve the fluidity and bonding performance of hot melt adhesives.

Benefits of technology

It achieves better elastic recovery performance of hot melt adhesive, low construction pressing temperature and excellent bonding performance, and improves the mechanical properties and light transmittance retention of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of copolyester hot melt adhesives, in particular to a copolyester hot melt adhesive and a preparation method thereof. The preparation method comprises the following steps: preparing modified 3-methyl adipic acid by adopting 3-methyl adipic acid, vinyltriethoxysilane and a free radical initiator as raw materials; the preparation method comprises the following steps: modifying nano powder by adopting a silane coupling agent to prepare a modified filler; according to the preparation method, the dibasic acid, the dihydric alcohol, the modified 3-methyl adipic acid, the modified filler and the auxiliary agent are further mixed to prepare the hot melt adhesive, and the hot melt adhesive prepared by the method has relatively good elastic recovery performance, relatively low construction pressing temperature and relatively good bonding performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copolyester hot melt adhesives, and in particular to a copolyester hot melt adhesive and a preparation method thereof. Background Art

[0002] Hot melt adhesive is a solid adhesive made of thermoplastic resin or thermoplastic elastomer as the main component, with plasticizer, tackifying resin, antioxidant, flame retardant and filler added, and then melted and mixed. The excellent properties of hot melt adhesive are: no solvent, 100% solid, no volatility, no pollution and no harm; easy to operate, can be cured in a short time; convenient to transport, can achieve continuous production and so on. This makes hot melt adhesive grow into the direction of development of the adhesive market, and its annual output is also steadily increasing.

[0003] Hot melt adhesives mainly include ethylene-vinyl acetate copolymer resins, polyethylene, random polypropylene, polyamide, polyester and polyurethane. Copolyester hot melt adhesive has high heat resistance, good water resistance and elasticity, and the polyester molecule contains -CO- bonds, which makes it have a good bonding effect on natural fibers such as wool, cotton, and linen and synthetic fibers such as polypropylene and polyester. It is widely used in the bonding of non-woven fabrics, carpet seams, clothing linings, zippers, etc. However, due to its high melt viscosity, poor fluidity and permeability, the single use of copolyester as the base polymer is difficult to meet the current actual needs, so the copolyester hot melt adhesive must be reasonably modified to meet the requirements of industrial production.

[0004] The Chinese patent with the announcement number CN117431031B discloses a copolyester hot melt adhesive and a preparation method thereof. The copolyester hot melt adhesive is composed of a composite copolyester, a cross-linking additive, 3-isocyanate propyltrimethoxysilane and an auxiliary additive. When the cross-linking additive and the composite copolyester are hot-melt mixed, under the action of the auxiliary catalyst zinc chloride, the oxirane group on the cross-linking additive can be promoted to open the ring, so that the epoxy ring cracks and reacts with the hydroxyl or amino active group on the composite copolyester to form a corresponding alcohol or amine cross-linking structure, thereby increasing the cross-linking degree of the hot melt adhesive, allowing the hot melt adhesive molecules to form more cross-linking points and cross-chain structures, and improving the bonding strength; the announcement number is CN112280 The Chinese patent No. 518B discloses an elastic copolyester hot melt adhesive and a preparation method thereof, wherein the main ingredients are composed of a dibasic acid and a diol, and the dibasic acid is a mixture of terephthalic acid and isophthalic acid in proportion; the diol is a mixture of 1,3-propylene glycol, 1,5-pentanediol and 1,7-heptanediol in proportion; the auxiliary materials include a catalyst, a stabilizer and an antioxidant; by using all the diols used in the copolyester hot melt adhesive system as odd-carbon diols and designing a unique material ratio, the copolyester hot melt adhesive prepared by the present invention has the advantages of a lower softening point suitable for gluing applications, good bonding and water-resistant properties to meet bonding requirements on the basis of good resilience. However, the above methods all directly add the raw materials during mixing, which will cause uneven mixing of the raw materials, thereby affecting product performance. Therefore, how to provide a copolyester hot melt adhesive so that the materials are more evenly dispersed during the mixing process and have better elasticity and better adhesion has become an urgent problem to be solved. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a copolyester hot melt adhesive and a preparation method thereof, which is prepared by mixing a dibasic acid, a diol, a modified 3-methyladipic acid, a modified filler and an auxiliary agent. The prepared copolyester hot melt adhesive has good elastic recovery performance, a lower construction pressing temperature and good bonding performance.

[0006] The technical solution adopted by the present invention to solve the above technical problems is: A method for preparing a copolyester hot melt adhesive, the preparation method comprising: S100, using 3-methyl adipic acid, vinyl triethoxysilane and a free radical initiator as raw materials to prepare modified 3-methyl adipic acid; S200, modifying the nano powder with a silane coupling agent to prepare a modified filler; S300, mixing a dibasic acid, a diol, a modified 3-methyl adipic acid, a modified filler and an auxiliary agent to prepare the hot melt adhesive.

[0007] Furthermore, step S100 specifically includes: S110, heating 3-methyladipic acid at 95-105° C. until it melts, to obtain molten 3-methyladipic acid; S120. Add a free radical initiator to molten 3-methyladipic acid, stir for 8-12 minutes, then add vinyltriethoxysilane, stir at a constant temperature for 15-25 minutes to obtain modified 3-methyladipic acid.

[0008] The purpose of step S100 is to prepare modified 3-methyladipic acid, and the preparation method is that vinyl triethoxysilane and 3-methyladipic acid are grafted under the action of a free radical initiator, and finally -CH2-, ethoxy and other groups are introduced into the prepared hot melt adhesive. The hot melt adhesive prepared after grafting is hydrolyzed and cross-linked under the action of moisture in the air or water molecules on the surface of the substrate, forming a cross-linked network inside the colloid, which increases the viscosity. At the same time, the presence of ethoxy groups can react with the hydroxyl groups on the surface of the bonding substrate to form chemical bonds, further improving the bonding strength. In addition, Si-O bonds are introduced into the hot melt adhesive system. Since its bond angle (140°) is greater than the bond angle of the CC bond (109.5°), the bond length (0.164nm) is greater than the CC bond length (0.154nm), and the oxygen atoms are saturated without any other substituents and atoms, the spacing between the non-bonding groups on adjacent silicon atoms in the Si-O-Si chain increases, and the internal rotation potential energy of the interaction decreases. Therefore, it can still rotate at low temperatures and has good softness, can entangle with the matrix molecular chains, and has good bonding properties.

[0009] Furthermore, in step S100, the free radical initiator is dicumyl peroxide; the mass ratio of 3-methyladipic acid, the free radical initiator and vinyltriethoxysilane is 20-35:1:15-22.

[0010] Furthermore, step S200 specifically includes: S210, drying the nano powder at 50-60° C. for 2-4 hours to obtain dry nano powder; S220, dissolving the dry nano powder and the silane coupling agent in anhydrous ethanol, placing the mixture at 85-95° C. and stirring for 20-40 minutes, filtering the mixture and drying it at 125-135° C. for 2-4 hours to obtain a modified filler.

[0011] The purpose of step S200 is to prepare a modified nano-silica filler, which is obtained by dissolving dried nano-silica and a silane coupling agent in anhydrous ethanol, stirring, filtering, and drying. Nano-silica is widely used in organic polymer materials as a reinforcing material, and can effectively improve the mechanical properties of the material. However, since the surface of nano-silica has abundant polar silanol groups, it is very easy to agglomerate. The special molecular structure of the silane coupling agent can form a "molecular bridge" at the interface between inorganic and organic substances, thereby improving the performance of the material and increasing the bonding strength. Therefore In the present invention, nano-silica is modified by a silane coupling agent, so that the active hydroxyl groups on the surface of the nano-silica can be reduced, the polarity of the particles can be weakened, the agglomeration of the particles can be reduced, the dispersion of the particles can be promoted, the compatibility between the inorganic particles and the organic polymer can be enhanced, and the mechanical properties can be improved; in addition, the nano-silica is a three-dimensional network particle with a porous structure, and the organic polymer chains can be interspersed in the pores of the powder, so that the inorganic and organic components are evenly dispersed into a unified whole, thereby improving the bonding strength; at the same time, the crystallinity of the hot melt adhesive is reduced to avoid the high crystallinity causing the hot melt adhesive to lose its elasticity as a whole, which is not conducive to bonding.

[0012] Further, in step S200, the nano powder is nano white carbon black, the silane coupling agent is KH560, and the mass ratio of the nano powder to the silane coupling agent is 10:0.2-0.4.

[0013] Furthermore, step S300 specifically includes: S310, adding dibasic acid, diol, modified 3-methyl adipic acid and catalyst into a reactor for esterification reaction, controlling the temperature to 165-215° C. and the pressure to 0.1-0.2 MPa, and when the amount of water generated by the reaction is more than 95% of the theoretical water output, the esterification reaction is terminated; S320, subjecting the product of step S310 to a reduced pressure polycondensation reaction at 225-235° C. and 30 Pa-60 Pa, and the polycondensation reaction is completed after 2-4 hours; S330, release the vacuum, add modified fillers and auxiliary agents, stir again under vacuum for 20-40 minutes, introduce nitrogen to release the vacuum, introduce it into the molding mold while it is hot, cool and solidify it to obtain the hot melt adhesive.

[0014] Polyester hot melt adhesive is based on polyester, and is a condensation product of aromatic acids such as terephthalic acid and isophthalic acid and diols such as ethylene glycol, butanediol, and diethylene glycol. However, it has high viscosity and is difficult to process, so how to improve its melt fluidity and make it easy to process becomes the key. The CC bond in the molecule of 3-methyladipic acid is easier to rotate than the benzene ring structure of terephthalic acid and isophthalic acid. In addition, the increase of 3-methyladipic acid can change the sequence distribution on the polyester molecular chain and increase the randomness of the chain segment, thereby increasing the flexibility of the polyester molecule and enhancing its fluidity; therefore, 3-methyladipic acid is selected to modify the polyester molecule. In order to further increase the bonding performance of the prepared hot melt adhesive, 3-methyladipic acid is modified using vinyl triethoxysilane. The presence of ethoxy in vinyl triethoxysilane can react with the hydroxyl group on the surface of the bonding substrate to form a chemical bond, further improving the bonding strength. Therefore, in the present invention, modified 3-methyladipic acid is used as a modified component and added to the preparation process of the copolyester hot melt adhesive, which can reduce the rigidity of the terephthalic acid-butylene isophthalate copolyester polymer chain, change its flexibility, crystallization rate and other characteristics, improve the melt fluidity when the hot melt adhesive is used, improve the wettability when bonding with the substrate, and improve the bonding performance of the hot melt adhesive.

[0015] Further, in step S300, the dibasic acid is a mixture of terephthalic acid and isophthalic acid, and the mass ratio of terephthalic acid to isophthalic acid is 1-3:1; the diol is 1,4-butanediol; and the catalyst is a mixture of butyl stannoic acid and tetrabutyl titanate, and the mass ratio of butyl stannoic acid to tetrabutyl titanate is 1:1.

[0016] Further, in step S300, the auxiliary agent is a mixture of a dispersant, a stabilizer and an antioxidant; the dispersant is zinc stearate; the stabilizer is triphenyl phosphite; and the antioxidant is one or more of 1010 antioxidant, 1076 antioxidant, 1135 antioxidant, 215 antioxidant, and 225 antioxidant.

[0017] The present invention also provides a copolyester hot melt adhesive, which is obtained by using the preparation method of any one of the above technical solutions.

[0018] The present invention has the following beneficial effects: The present invention uses dibasic acid, diol, modified 3-methylhexanedioic acid, modified filler and auxiliary agent as raw materials to prepare copolyester hot melt adhesive. Modified 3-methylhexanedioic acid is obtained by grafting reaction of 3-methylhexanedioic acid and vinyl triethoxysilane under the action of free radical initiator. The introduced -CH2-, ethoxyl and other groups can be hydrolyzed and cross-linked under the action of water molecules, forming a cross-linked network inside the colloid, so that the viscosity of the hot melt adhesive is increased; on the other hand, the presence of ethoxyl group can also react with hydroxyl groups on the surface of the bonding substrate to generate chemical bonds, further improving the bonding strength; in addition, the introduction of Si-O bond and CC can increase the flexibility of polyester molecules and enhance their fluidity. At the same time, nano-silica modified by silane coupling agent is also added in the preparation process of hot melt adhesive. Nano-silica as inorganic particles can effectively improve the mechanical properties of materials; at the same time, nano-silica is a three-dimensional mesh particle with a porous structure, and organic polymer chains can be interspersed in the pores of the powder, so that inorganic and organic components are evenly dispersed into a unified whole, improving the bonding strength and reducing the crystallinity of polyester. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0020] 3-Methyladipic acid (code XW02305801301), vinyl triethoxysilane (code 80149328), zinc stearate (code 30193128), and triphenyl phosphite (code 30187628) used in the present invention are all purchased from Sinopharm Chemical Reagent Co., Ltd., nano-silica gel is purchased from Huizhou Huayan Industrial Co., Ltd., terephthalic acid (industrial grade) and isophthalic acid (industrial grade) are purchased from Shanghai Bangcheng Chemical Co., Ltd., 1,4-butanediol (industrial grade) is purchased from Shanxi Sanwei Co., Ltd., butyl stannoic acid (analytical grade) and tetrabutyl titanate (analytical grade) are purchased from Shanghai Chemical Reagent Co., Ltd.; all reagents are commercially available.

[0021] Embodiment 1 A method for preparing a copolyester hot melt adhesive, the preparation method comprising: S100, using 3-methyl adipic acid, vinyl triethoxysilane and a free radical initiator as raw materials to prepare modified 3-methyl adipic acid; S200, modifying the nano powder with a silane coupling agent to prepare a modified filler; S300, mixing dibasic acid, diol, modified 3-methyl adipic acid, modified filler and auxiliary agent to prepare hot melt adhesive.

[0022] Wherein, step S100 specifically includes: S110, heating 3-methyladipic acid at 100° C. until it melts, to obtain molten 3-methyladipic acid; S120. Add a free radical initiator to molten 3-methyladipic acid, stir for 10 minutes, then add vinyltriethoxysilane, stir at a constant temperature for 20 minutes to obtain modified 3-methyladipic acid.

[0023] Wherein, in step S100, the free radical initiator is dicumyl peroxide; the mass ratio of 3-methyladipic acid, the free radical initiator and vinyltriethoxysilane is 25:1:20.

[0024] Wherein, step S200 specifically includes: S210, drying the nano powder at 55° C. for 3 h to obtain dry nano powder; S220, dissolving the dry nano powder and the silane coupling agent in anhydrous ethanol, stirring at 90° C. for 30 min, filtering and drying at 130° C. for 3 h to obtain a modified filler.

[0025] Wherein, in step S200, the nano powder is nano silica, the silane coupling agent is KH560, the mass ratio of the nano powder to the silane coupling agent is 10:0.3, and the amount of nano silica in anhydrous ethanol is 1.2 g / mL.

[0026] Wherein, step S300 specifically includes: S310, adding 192g of terephthalic acid, 80g of isophthalic acid, 225g of 1,4-butanediol, 265g of modified 3-methyladipic acid, 0.02g of butyl stannoic acid and 0.02g of tetrabutyl titanate into a reactor for esterification reaction, gradually heating to 165°C, maintaining the pressure in the reactor at 0.1-0.2MPa, starting stirring, when the temperature approaches 185°C, water begins to distill out, continuing to gradually heat to 215°C, and the esterification reaction is completed when the water output is more than 95% of the theoretical water output; S320, gradually heating the product of step S310 to 230°C and keeping the temperature, gradually reducing the pressure in the reactor to 60Pa, and maintaining the temperature for 3h before the polycondensation reaction is completed; S330, release the vacuum, add 25g of modified nano-white carbon black, 0.02g of zinc stearate, 0.02g of triphenyl phosphite and 0.02g of 1010 antioxidant, re-evacuate and stir for 30min, introduce nitrogen to release the vacuum, introduce it into the molding mold while it is hot, cool and solidify to obtain the hot melt adhesive.

[0027] Embodiment 2 Compared with the first embodiment, this embodiment has the following differences: Step S100: In step S110, 3-methyl adipic acid is heated at 95°C until it melts to obtain molten 3-methyl adipic acid; in step S120, a free radical initiator is added to the molten 3-methyl adipic acid, and after stirring for 8 minutes, vinyl triethoxysilane is added thereto, and stirred at a constant temperature for 15 minutes to obtain modified 3-methyl adipic acid; wherein the mass ratio of 3-methyl adipic acid, free radical initiator and vinyl triethoxysilane is 20:1:15.

[0028] Step S200: In step S210, the nanopowder is dried at 50°C for 2 hours to obtain dry nanopowder; in step S220, the dry nanopowder and the silane coupling agent are dissolved in anhydrous ethanol, stirred at 85°C for 20 minutes, filtered and dried at 125°C for 2 hours to obtain a modified filler; wherein the mass ratio of the nanopowder to the silane coupling agent is 10:0.2, and the amount of nano-white carbon black in anhydrous ethanol is 1.0 g / mL.

[0029] Step S300: In step S310, 160g of terephthalic acid, 80g of isophthalic acid, 200g of 1,4-butanediol, 235g of modified 3-methyladipic acid, 0.012g of butyl stannoic acid and 0.012g of tetrabutyl titanate are added to the reaction kettle for esterification reaction, and the temperature is gradually raised to 165°C, the pressure in the kettle is maintained at 0.1-0.2MPa, stirring is turned on, and when the temperature approaches 185°C, water begins to distill out, and the temperature is gradually raised to 215°C. When the water output is more than 95% of the theoretical water output, esterification is completed. The reaction is over; in step S320, the product of step S310 is gradually heated to 225°C and kept warm, the pressure in the reactor is gradually reduced to 60 Pa, and maintained for 2 hours before the polycondensation reaction is completed; in step S330, the vacuum is released, 20g of modified nano-white carbon black, 0.012g of zinc stearate, 0.012g of triphenyl phosphite and 0.012g of 1010 antioxidant are added, the vacuum is re-drawn and stirred for 20 minutes, nitrogen is introduced to release the vacuum, and it is introduced into the molding mold while hot, cooled and solidified to obtain the hot melt adhesive.

[0030] The rest is as per Example 1.

[0031] Embodiment 3 Compared with the first embodiment, this embodiment has the following differences: Step S100: In step S110, 3-methyl adipic acid is heated at 105°C until it is melted to obtain molten 3-methyl adipic acid; in step S120, a free radical initiator is added to the molten 3-methyl adipic acid, and after stirring for 12 minutes, vinyl triethoxysilane is added thereto, and stirred at a constant temperature for 25 minutes to obtain modified 3-methyl adipic acid; wherein the mass ratio of 3-methyl adipic acid, free radical initiator and vinyl triethoxysilane is 35:1:22.

[0032] Step S200: In step S210, the nanopowder is dried at 60°C for 4 hours to obtain dry nanopowder; in step S220, the dry nanopowder and the silane coupling agent are dissolved in anhydrous ethanol, stirred at 95°C for 40 minutes, filtered and dried at 135°C for 4 hours to obtain a modified filler; wherein the mass ratio of the nanopowder to the silane coupling agent is 10:0.4, and the amount of nano-white carbon black in anhydrous ethanol is 1.4 g / mL.

[0033] Step S300: In step S310, 240g of terephthalic acid, 80g of isophthalic acid, 255g of 1,4-butanediol, 280g of modified 3-methyladipic acid, 0.025g of butyl stannoic acid and 0.025g of tetrabutyl titanate are added to a reaction kettle for esterification reaction, and the temperature is gradually raised to 165°C, the pressure in the kettle is maintained at 0.1-0.2MPa, stirring is turned on, and when the temperature approaches 185°C, water begins to distill out, and the temperature is gradually raised to 215°C. When the water output is more than 95% of the theoretical water output, esterification is carried out. The reaction is over; in step S320, the product of step S310 is gradually heated to 235°C and kept warm, the pressure in the reactor is gradually reduced to 60Pa, and maintained for 4 hours before the polycondensation reaction is completed; in step S330, the vacuum is released, 30g of modified nano-white carbon black, 0.025g of zinc stearate, 0.025g of triphenyl phosphite and 0.025g of 1010 antioxidant are added, the vacuum is re-drawn and stirred for 30 minutes, nitrogen is introduced to release the vacuum, and it is introduced into the molding mold while hot, cooled and solidified to obtain a hot melt adhesive.

[0034] The rest is as per Example 1.

[0035] Comparative Example 1 Compared with Example 1, in this comparative example, 3-methyl adipic acid is not modified during the preparation of the hot melt adhesive, and 3-methyl adipic acid is directly added to modify the polyester hot melt adhesive. The rest is referred to Example 1, which is as follows: A method for preparing a copolyester hot melt adhesive, the preparation method comprising: S10, modifying the nanopowder with a silane coupling agent to prepare a modified filler; S20, mixing the dibasic acid, diol, 3-methyladipic acid, modified filler and auxiliary agent to prepare a hot melt adhesive.

[0036] Wherein, step S1 specifically includes: S11, drying the nano powder at 55° C. for 3 h to obtain dry nano powder; S12, dissolving the dry nano powder and the silane coupling agent in anhydrous ethanol, placing the mixture under constant temperature stirring at 90° C. for 30 min, filtering the mixture, and drying the mixture at 130° C. for 3 h to obtain a modified filler.

[0037] Wherein, in step S10, the nano powder is nano silica, the silane coupling agent is KH560, the mass ratio of the nano powder to the silane coupling agent is 10:0.3, and the amount of nano silica in anhydrous ethanol is 1.2 g / mL.

[0038] Wherein, step S20 specifically includes: S21, 192g of terephthalic acid, 80g of isophthalic acid, 300g of 1,4-butanediol, 265g of 3-methyladipic acid, 0.02g of butyl stannoic acid and 0.02g of tetrabutyl titanate are added to a reactor for esterification reaction, and the temperature is gradually raised to 165°C, the pressure in the reactor is maintained at 0.1-0.2MPa, stirring is turned on, and when the temperature approaches 185°C, water begins to distill out, and the temperature is gradually raised to 215°C. The esterification reaction is completed when the water output is more than 95% of the theoretical water output; S22, gradually heating the product of step S21 to 230°C and keeping the temperature, gradually reducing the pressure in the reactor to 60Pa, and maintaining the temperature for 3h before the polycondensation reaction is completed; S23, release the vacuum, add 25g of modified nano-white carbon black, 0.02g of zinc stearate, 0.02g of triphenyl phosphite and 0.02g of 1010 antioxidant, re-evacuate and stir for 30min, introduce nitrogen to release the vacuum, introduce it into the molding mold while it is hot, cool and solidify to obtain the hot melt adhesive.

[0039] Comparative Example 2 Compared with Example 1, the nano powder is not modified in this comparative example, and the rest is referred to Example 1, which is as follows: A method for preparing a copolyester hot melt adhesive, the preparation method comprising: S10, using 3-methyl adipic acid, vinyl triethoxysilane and a free radical initiator as raw materials to prepare modified 3-methyl adipic acid; S20, mixing the dibasic acid, diol, modified 3-methyladipic acid, filler and auxiliary agent to prepare a hot melt adhesive.

[0040] Wherein, step S1 specifically includes: S11, heating 3-methyladipic acid at 100° C. until it melts, to obtain molten 3-methyladipic acid; S12. Add a free radical initiator to molten 3-methyladipic acid, stir for 10 minutes, then add vinyltriethoxysilane, stir at a constant temperature for 20 minutes to obtain modified 3-methyladipic acid.

[0041] Wherein, in step S1, the free radical initiator is dicumyl peroxide; the mass ratio of 3-methyladipic acid, the free radical initiator and vinyltriethoxysilane is 25:1:20.

[0042] Wherein, the filler in step S20 is nano-white carbon black.

[0043] Wherein, step S20 specifically includes: S21, 192g of terephthalic acid, 80g of isophthalic acid, 225g of 1,4-butanediol, 265g of modified 3-methyladipic acid, 0.02g of butyl stannoic acid and 0.02g of tetrabutyl titanate are added to a reactor for esterification reaction, and the temperature is gradually raised to 165°C, the pressure in the reactor is maintained at 0.1-0.2MPa, stirring is turned on, and when the temperature approaches 185°C, water begins to distill out, and the temperature is gradually raised to 215°C. The esterification reaction is terminated when the water output is more than 95% of the theoretical water output; S22, gradually heating the product of step S21 to 230°C and keeping the temperature, gradually reducing the pressure in the reactor to 60Pa, and maintaining the temperature for 3h before the polycondensation reaction is completed; S23, release the vacuum, add 25g of nano-white carbon black, 0.02g of zinc stearate, 0.02g of triphenyl phosphite and 0.02g of 1010 antioxidant, re-evacuate and stir for 30min, introduce nitrogen to release the vacuum, introduce it into the molding mold while it is hot, cool and solidify to obtain the hot melt adhesive.

[0044] Comparative Example 3 Compared with Example 1, this comparative example does not add modified filler during the preparation of the hot melt adhesive, and the rest is referred to Example 1, specifically: A method for preparing a copolyester hot melt adhesive, the preparation method comprising: S10, using 3-methyl adipic acid, vinyl triethoxysilane and a free radical initiator as raw materials to prepare modified 3-methyl adipic acid; S20, mixing the dibasic acid, diol, modified 3-methyladipic acid and an auxiliary agent to prepare a hot melt adhesive.

[0045] Wherein, step S10 specifically includes: S11, heating 3-methyladipic acid at 100° C. until it melts, to obtain molten 3-methyladipic acid; S12. Add a free radical initiator to molten 3-methyladipic acid, stir for 10 minutes, then add vinyltriethoxysilane, stir at a constant temperature for 20 minutes to obtain modified 3-methyladipic acid.

[0046] Wherein, in step S10, the free radical initiator is dicumyl peroxide; the mass ratio of 3-methyladipic acid, the free radical initiator and vinyltriethoxysilane is 25:1:20.

[0047] Wherein, step S20 specifically includes: S21, 192g of terephthalic acid, 80g of isophthalic acid, 225g of 1,4-butanediol, 265g of modified 3-methyladipic acid, 0.02g of butyl stannoic acid and 0.02g of tetrabutyl titanate are added to a reactor for esterification reaction, and the temperature is gradually raised to 165°C, the pressure in the reactor is maintained at 0.1-0.2MPa, stirring is turned on, and when the temperature approaches 185°C, water begins to distill out, and the temperature is gradually raised to 215°C. The esterification reaction is terminated when the water output is more than 95% of the theoretical water output; S22, gradually heating the product of step S21 to 230°C and keeping the temperature, gradually reducing the pressure in the reactor to 60Pa, and maintaining the temperature for 3h before the polycondensation reaction is completed; S23, release the vacuum, add 0.02g zinc stearate, 0.02g triphenyl phosphite and 0.02g 1010 antioxidant, re-evacuate and stir for 30min, introduce nitrogen to release the vacuum, introduce it into the molding mold while it is hot, cool and solidify to obtain the hot melt adhesive.

[0048] Comparative Example 4 Compared with Example 1, in this comparative example, modified 4-methyladipic acid and modified filler are not added during the preparation of the hot melt adhesive, and the rest is referred to Example 1, specifically: A method for preparing a copolyester hot melt adhesive, the method comprising: mixing a dibasic acid, a diol and an auxiliary agent to prepare a hot melt adhesive; specifically: S1. Add 192g of terephthalic acid, 80g of isophthalic acid, 155g of 1,4-butanediol, 0.02g of butyl stannoic acid and 0.02g of tetrabutyl titanate into a reactor for esterification reaction. Gradually raise the temperature to 165°C, maintain the pressure in the reactor at 0.1-0.2MPa, start stirring, and when the temperature approaches 185°C, water begins to distill out. Continue to gradually raise the temperature to 215°C, and the esterification reaction is completed when the water output is more than 95% of the theoretical water output; S2, gradually heating the product of step S1 to 230°C and keeping the temperature, gradually reducing the pressure in the reactor to 60Pa, and maintaining the temperature for 3h before the polycondensation reaction is completed; S3, release the vacuum, add 0.02g zinc stearate, 0.02g triphenyl phosphite and 0.02g 1010 antioxidant, re-evacuate and stir for 30min, then introduce nitrogen to release the vacuum, introduce it into the molding mold while it is hot, cool and solidify to obtain the hot melt adhesive.

[0049] Related performance tests According to the standard GB / T 16998-1997 "Determination of thermal stability of hot-melt adhesives", the melt viscosity and softening temperature of the hot-melt adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were measured, and the hot-melt adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were heated and melted using a hot-melt device, and then uniformly coated on the surface of the transparent glass. The transparent glass coated with the hot-melt adhesive was placed in a room temperature environment with a humidity of 45% for curing and curing for 10 hours, and an adhesive layer with a thickness of 0.2±0.02 mm was formed on the glass surface. The 180° peel strength of the adhesive layer was measured according to the standard GB / T 2790-1995 "Test method for 180° peel strength of adhesives - flexible material to rigid material", and the light transmittance of the transparent glass sample coated with the hot-melt adhesive and the transparent glass was measured according to the standard JB / T 9495.3-1999 "Measurement method for transmittance of optical crystals", and the formula (λ 试样的透光率 / λ 透明玻璃的透光率 )×100% to measure the light transmittance retention rate of the sample after coating with hot melt adhesive. The transparent glass sample coated with hot melt adhesive was placed in a test box with a humidity of 50% and a temperature of 70°C, and irradiated with a UV-B fluorescent lamp. The irradiation intensity on the sample surface was 50W / m 2 The samples were exposed in the test box for 48 hours for aging test, and the 180° peel strength and light transmittance retention rate of the samples were measured and calculated. The specific test results are shown in Table 1.

[0050] Table 1 Related performance tests The above experimental results show that the melt viscosity of the hot melt adhesive prepared by the present invention is maintained at about 4800 mPa·s, and the softening temperature is between 115°C and 123°C, which can make it have a lower pressing temperature and is suitable for industrial applications. The 180° peel strength is maintained at 27.85 N·15 mm. -1 , the light transmittance retention rate reached 97.25%; after aging test, the 180° peel strength remained at 26.86N·15mm -1 , the light transmittance retention rate reaches 96.35%, which indicates that the hot melt adhesive prepared by the present invention has lower melt viscosity and softening temperature, and improves its peel strength, light transmittance and antioxidant properties.

[0051] Related mechanical property tests: The hot melt adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to elastic recovery performance tests (tensile recovery rate at a fixed elongation of 200%) according to ASTM D2594-2004 (2012); the elongation at break was determined according to GB / T 13022-1991; the test results are shown in Table 2.

[0052] Table 2 Related mechanical properties It can be seen from the test results in Table 2 that the hot melt adhesive prepared by the present invention has high elastic properties, its fixed elongation recovery rate is maintained at about 80%, and its elongation at break is maintained at about 730%. Combining the test data in Tables 1 and 2, it can be seen that the hot melt adhesive prepared by the present invention has good elastic recovery performance, low construction pressing temperature and good bonding performance.

[0053] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0054] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a copolyester hot melt adhesive, characterized in that: The preparation method comprises: S100, using 3-methyl adipic acid, vinyl triethoxysilane and a free radical initiator as raw materials to prepare modified 3-methyl adipic acid; S200, modifying the nano powder with a silane coupling agent to prepare a modified filler; S300, mixing a dibasic acid, a diol, a modified 3-methyl adipic acid, a modified filler and an auxiliary agent to prepare the hot melt adhesive.

2. The preparation method according to claim 1, characterized in that: Step S100 specifically includes: S110, heating 3-methyladipic acid at 95-105° C. until it melts, to obtain molten 3-methyladipic acid; S120. Add a free radical initiator to molten 3-methyladipic acid, stir for 8-12 minutes, then add vinyltriethoxysilane, stir at a constant temperature for 15-25 minutes to obtain modified 3-methyladipic acid.

3. The preparation method according to claim 2, characterized in that: The free radical initiator is dicumyl peroxide; the mass ratio of 3-methyladipic acid, the free radical initiator and vinyl triethoxysilane is 20-35:1:15-22.

4. The preparation method according to claim 1, characterized in that: Step S200 specifically includes: S210, drying the nano powder at 50-60° C. for 2-4 hours to obtain dry nano powder; S220, dissolving the dry nano powder and the silane coupling agent in anhydrous ethanol, placing the mixture at 85-95° C. and stirring for 20-40 minutes, filtering the mixture and drying it at 125-135° C. for 2-4 hours to obtain a modified filler.

5. The preparation method according to claim 4, characterized in that: The nano powder is nano white carbon black, the silane coupling agent is KH560, and the mass ratio of the nano powder to the silane coupling agent is 10:0.2-0.

4.

6. The preparation method according to claim 1, characterized in that: Step S300 specifically includes: S310, adding dibasic acid, diol, modified 3-methyl adipic acid and catalyst into a reactor for esterification reaction, controlling the temperature to 165-215° C. and the pressure to 0.1-0.2 MPa, and when the amount of water generated by the reaction is more than 95% of the theoretical water output, the esterification reaction is terminated; S320, subjecting the product of step S310 to a reduced pressure polycondensation reaction at 225-235° C. and 30 Pa-60 Pa, and the polycondensation reaction is completed after 2-4 hours; S330, release the vacuum, add modified fillers and auxiliary agents, stir again under vacuum for 20-40 minutes, introduce nitrogen to release the vacuum, introduce it into the molding mold while it is hot, cool and solidify it to obtain the hot melt adhesive.

7. The preparation method according to claim 6, characterized in that: The dibasic acid is a mixture of terephthalic acid and isophthalic acid, and the mass ratio of terephthalic acid to isophthalic acid is 1-3:1; the diol is 1,4-butanediol; and the catalyst is a mixture of butyl stannoic acid and tetrabutyl titanate, and the mass ratio of butyl stannoic acid to tetrabutyl titanate is 1:

1.

8. The preparation method according to claim 6, characterized in that: The auxiliary agent is a mixture of a dispersant, a stabilizer and an antioxidant; the dispersant is zinc stearate; the stabilizer is triphenyl phosphite; and the antioxidant is one or more of 1010 antioxidant, 1076 antioxidant, 1135 antioxidant, 215 antioxidant and 225 antioxidant.

9. A copolyester hot melt adhesive, characterized in that: The copolyester hot melt adhesive is obtained by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Modified polyamide thermosol based on polyester and preparation thereof

    CN101463244A

  • Elastic copolyester hot melt adhesive and preparation method thereof

    CN112280518A

  • Hot melt adhesive raw material, preparation method of hot melt adhesive raw material, heat-shrinkable sleeve and manufacturing method of heat-shrinkable sleeve

    CN117070163A

  • High-performance polyester hot melt adhesive and preparation method thereof

    CN118703150A