Color-adjustable storage-resistant two-component silicone structural sealant and preparation method thereof

By optimizing the components and preparation process of two-component silicone structural sealant, combined with pretreatment and dehydration of color paste, the problems of single glue color and unstable viscosity curing time are solved, and the richness of colloid color is achieved and storage stability, suitable for multi-field applications.

CN118931475APending Publication Date: 2024-11-12CHENGDU GUIBAO SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411057581.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The two-component silicone structural sealant on the market has a single color, which cannot meet the different color needs of customers. The viscosity and curing time are insufficient, making it difficult to meet the needs of different fields.

Method used

Two-component silicone structure sealant with a mass ratio of 13 to 15:1 of component A and component B. Component A includes α,ω-dihydroxypolydimethylsiloxane, active nano calcium carbonate and Heavy calcium carbonate, component B includes polyalkoxy-terminated polydimethylsiloxane, toning pigment, hydrophobic white carbon black, silicone rubber two-component vulcanizing agent and accelerator, through toning chromatic paste Pretreatment and dehydration to ensure rich colloid color and stable storage.

Benefits of technology

It realizes the richness of colloid color, viscosity and curing time stability, is suitable for applications in multiple fields, has good adhesion and aging resistance, and is suitable for building and structural bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004976876250000091
    Figure BDA0004976876250000091
  • Figure BDA0004976876250000101
    Figure BDA0004976876250000101
  • Figure BDA0004976876250000102
    Figure BDA0004976876250000102
Patent Text Reader

Abstract

The invention relates to the technical field of double-component silicone sealants, and discloses a color-adjustable and storage-resistant double-component silicone structural sealant and a preparation method thereof.The sealant comprises a component A and a component B. The weight ratio of the component A to the component B is 13: 1-15: 1. Color-adjusting color paste in the component B is pretreated, a vulcanizing agent and an accelerant are pretreated, and therefore the color-adjustable and storage-resistant double-component silicone structural sealant is obtained. And the hydrophobic white carbon black is used, so that compared with the prior art, the material has better mechanical properties, also has the advantages of stable curing time and stable viscosity after storage, is very suitable for field engineering with different color requirements, has good cohesiveness and excellent aging resistance, and can be widely applied to the field of engineering with different color requirements. And the adhesive is also suitable for bonding related structures in constructional engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of two-component silicone sealants, and in particular to a color-adjustable and storage-resistant two-component silicone structural sealant and a preparation method thereof. Background Art

[0002] Silicone structural sealant is a high-performance special adhesive, mainly used in construction, automobiles, aerospace, electronics, new energy and other fields. Its main characteristics include: 1. High bonding strength: Silicone structural sealant can provide high-strength bonding effect and effectively resist the adverse effects of various environmental factors on materials. 2. Excellent weather resistance: It has excellent weather resistance, can maintain stable performance in various harsh environments, and is not easily affected by ultraviolet rays, temperature changes, humidity and other factors. 3. Good curing effect: During the curing process, the shrinkage rate of silicone structural sealant is low, and the volume is stable after curing. It is not easy to have bubbles, cracks and other phenomena, ensuring a good sealing effect. 4. Elasticity and toughness: After curing, silicone structural sealant forms elastic silicone rubber, which has good elasticity and toughness and can withstand a certain degree of displacement and vibration. 5. Chemical stability: It has good adhesion to most building materials and is not affected by sunlight, rain, wind and snow and extreme temperatures, showing good chemical stability.

[0003] Although silicone structural sealants have many advantages, the two-component silicone structural sealants on the market still have the following problems: the color of the glue is single, which cannot meet the different needs of customers for the color of the glue; and the use time and operation time of the glue process are different in different glue application fields, so stable viscosity performance and curing time are required. In summary, how to enrich the colloid color of the two-component silicone structural sealant while ensuring the stability of its viscosity and tear and surface drying time is of great significance. Summary of the invention

[0004] The present invention aims to provide a color-adjustable and storage-resistant two-component silicone structural sealant and a preparation method, which can enrich the color of the colloid and ensure the stability of viscosity, tearing time and surface drying time during storage.

[0005] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a color-adjustable and storage-resistant two-component silicone structural sealant, comprising component A and component B, the mass ratio of component A to component B being 13-15:1; component A comprising the following raw materials in mass ratio: 100 parts of α,ω-dihydroxy polydimethylsiloxane, 20-40 parts of dimethyl silicone oil, 80-100 parts of active nano-calcium carbonate, and 10-30 parts of heavy calcium carbonate; component B comprising the following raw materials in mass ratio: 100 parts of polyalkoxy-terminated polydimethylsiloxane, 30-60 parts of dimethyl silicone oil, 10-30 parts of coloring pigment, 30-50 parts of hydrophobic white carbon black, 60-80 parts of silicone rubber two-component vulcanizer, 1-2 parts of stabilizer, 0.5-1 part of accelerator, and 1-2 parts of catalyst.

[0006] Preferably, as an improvement, the viscosity of α,ω-dihydroxypolydimethylsiloxane at 25°C is 10000-50000 mPa·s; the viscosity of dimethyl silicone oil at 25°C is 100-350 mPa·s.

[0007] Preferably, as an improvement, the particle size of the active nano calcium carbonate is 800-1200 mesh; the particle size of the heavy calcium carbonate is 100-200 mesh.

[0008] Preferably, as an improvement, the viscosity of the polyalkoxy-terminated polydimethylsiloxane at 25° C. is 1500 to 20000 mPa·s; the specific surface area of ​​the hydrophobic silica is 150 to 200 m 2 / g.

[0009] Preferably, as an improvement, the two-component vulcanizing agent for silicone rubber is composed of at least two of ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, and phenyltriethoxysilane, and at least two of dimethyldimethoxysilane, diethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and N-β-(aminoethyl)γ-aminopropyltriethoxysilane.

[0010] Preferably, as an improvement, the catalyst is one of dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin acetate; and the promoter is one of sodium isooctanoate, zinc isooctanoate, and lithium isooctanoate.

[0011] Preferably, as an improvement, the coloring pigment is composed of at least three of medium chrome yellow, scarlet, iron red, brilliant red, carbon black, phthalocyanine blue, phthalocyanine green and titanium white.

[0012] Preferably, as an improvement, the stabilizer is isocyanate methyltrimethoxysilane.

[0013] Preferably, as an improvement, a method for preparing a color-adjustable and storage-resistant two-component silicone structural sealant comprises the following steps:

[0014] Step 1, preparing component A: stirring α,ω-dihydroxy polydimethylsiloxane, dimethyl silicone oil, active nano calcium carbonate and heavy calcium carbonate evenly;

[0015] Step 2: Preparation of component B:

[0016] S1. Preparation of color paste: polyalkoxy-terminated polydimethylsiloxane, dimethyl silicone oil, and color pigment are stirred evenly, and then isocyanate methyl trimethoxy silane is added. After sufficient stirring, the mixture is heated, dehydrated, and cooled for use;

[0017] S2. Pretreatment of the two-component vulcanizer and accelerator of silicone rubber: after the two-component vulcanizer and accelerator of silicone rubber are mixed, heated and stirred, and then cooled;

[0018] S3. Preparation of component B: Mix the color paste, the pre-treated silicone rubber two-component vulcanizer and accelerator, and the catalyst evenly to obtain component B.

[0019] Step 3. Preparation of sealant: When using, mix component A and component B at a mass ratio of 13 to 15:1, degas, and cure at room temperature.

[0020] Preferably, as an improvement, in step one, the stirring conditions are: first stirring at normal pressure for 30 minutes, then stirring under vacuum for 60 minutes at a temperature of 80 to 90° C. and a vacuum degree of -0.08 to 0.099 MPa, and then cooling.

[0021] Preferably, as an improvement, in step 2, the heating temperature of S2 is 40-60° C., and the stirring time is 2 h; in S3, the stirring conditions are room temperature and vacuum degree -0.08-0.099 MPa.

[0022] The principle and advantages of this solution are: in actual application, in this technical solution, the components and preparation process of the two-component silicone sealant are optimized as a whole in view of the problems existing in the prior art, the coloring paste is pretreated in the B component, and hydrophobic white carbon black is used in the preparation of the B component coloring paste, and a stabilizer is added and dehydration treatment is performed, so that the properties of the B component can ensure storage stability after adding different pigments, so that the viscosity and curing time of the B component will not change greatly. In addition, the technical solution pre-treats the vulcanizer and the accelerator, and uses hydrophobic white carbon black, so that it has better mechanical properties, and also has the advantages of stable curing time and stable viscosity after storage, which is very suitable for field projects with different color requirements. At the same time, good adhesion and excellent aging resistance are also suitable for the bonding of related structures in construction projects. In the technical research and development stage, in order to achieve the purpose of color adjustment, the B component needs to be made into a colorless or white state, so the reinforcing raw material used is white carbon black. However, the terminal hydroxyl groups on the surface of hydrophilic silica are highly active and easy to absorb water. If the dehydration treatment and removal of active groups are not thorough, component B will thicken and cannot be stored for a long time. At this time, the use of hydrophobic silica reduces water absorption and has fewer surface hydroxyl groups. The use of polyalkoxy-terminated polydimethylsiloxane further increases storage stability. In addition, the technical solution first reacts the vulcanizing agent and the accelerator to eliminate hydroxyl groups and heteroactive groups, making the entire reaction system more stable. Since there is a risk of thickening when too much water contacts the material, the separate preparation of the vulcanizing agent and the accelerator can also avoid the multiple addition of additives during the preparation of the sealant and reduce excessive water contact with the material during the glue making process.

[0023] In summary, compared with the prior art inventions, the beneficial effects of the present invention are: under the condition of satisfying the richness of the colloid color, it ensures stable bonding, good aging resistance and temperature resistance in the application process in multiple fields, which is of great significance for being able to widely meet the gluing stability in multiple fields. DETAILED DESCRIPTION

[0024] The following is further described in detail through specific implementations, but the implementation of the present invention is not limited thereto. Unless otherwise specified, the technical means used in the following implementations are conventional means well known to those skilled in the art; the experimental methods used are all conventional methods; the materials, reagents, etc. used can all be obtained from commercial channels.

[0025] Program Overview:

[0026] A color-adjustable and storage-resistant two-component silicone structural sealant comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 13-15:1, and the component A comprises the following raw materials in the following mass ratios: 100 parts of α,ω-dihydroxy polydimethylsiloxane, 20-40 parts of dimethyl silicone oil, 80-100 parts of active nano calcium carbonate, and 10-30 parts of heavy calcium carbonate;

[0027] Among them, the viscosity of α,ω-dihydroxy polydimethylsiloxane at 25°C is 10000-50000 mPa·s; the viscosity of dimethyl silicone oil at 25°C is 100-350 mPa·s; the particle size of active nano calcium carbonate is 800-1200 mesh; the particle size of heavy calcium carbonate is 100-200 mesh;

[0028] Component B includes the following raw materials in mass ratio: 100 parts of polyalkoxy-terminated polydimethylsiloxane, 30-60 parts of dimethyl silicone oil, 10-30 parts of color pigment, 30-50 parts of hydrophobic white carbon black, 60-80 parts of silicone rubber two-component vulcanizer, 1-2 parts of stabilizer, 0.5-1 part of accelerator, and 1-2 parts of catalyst;

[0029] The viscosity of the polyalkoxy-terminated polydimethylsiloxane at 25° C. is 1500 to 20000 mPa·s; the coloring pigment is composed of at least three of medium chrome yellow, scarlet, iron red, brilliant red, carbon black, phthalocyanine blue, phthalocyanine green, and titanium dioxide; the specific surface area of ​​the hydrophobic white carbon black is 150 to 200 m 2 / g; the two-component vulcanizing agent for silicone rubber is composed of at least two of ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, and phenyltriethoxysilane, and at least two of dimethyldimethoxysilane, diethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and N-β-(aminoethyl)γ-aminopropyltriethoxysilane; the stabilizer is isocyanate methyltrimethoxysilane; the catalyst is one of dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin acetate; the accelerator is one of sodium isooctanoate, zinc isooctanoate, and lithium isooctanoate.

[0030] A method for preparing a color-adjustable and storage-resistant two-component silicone structural sealant comprises the following steps:

[0031] Step 1, prepare component A: put α, ω-dihydroxy polydimethylsiloxane, dimethyl silicone oil, active nano calcium carbonate and heavy calcium carbonate into a high-speed disperser, stir at normal pressure for 30 minutes, then stir under vacuum for 60 minutes at a temperature of 80 to 90°C and a vacuum degree of -0.08 to 0.099 MPa, and cool to obtain.

[0032] Step 2: Preparation of component B:

[0033] S1. Preparation of color paste: polyalkoxy-terminated polydimethylsiloxane, dimethyl silicone oil, and color pigment, stir evenly, add isocyanate methyl trimethoxysilane, stir thoroughly for 1 hour, heat to 110-130° C., dehydrate for 2 hours, cool and set aside;

[0034] S2. Pretreatment of two-component vulcanizer and accelerator of silicone rubber: After mixing the two-component vulcanizer and accelerator of silicone rubber, stir them thoroughly at 40-60°C for 2h, then cool to room temperature (25°C), seal and store for later use.

[0035] S3. Preparation of component B: put the above-obtained color paste, pre-treated silicone rubber two-component vulcanizer and accelerator, and catalyst into a high-speed disperser, and stir evenly at room temperature and vacuum degree of -0.08 to 0.099 MPa to obtain component B.

[0036] Step 3. Preparation of sealant: When using, mix component A and component B at a mass ratio of 13 to 15:1, degas, and cure at room temperature.

[0037] Example 1

[0038] A method for preparing a color-adjustable and storage-resistant two-component silicone structural sealant comprises the following steps:

[0039] Step 1, prepare component A: put 100 parts of α,ω-dihydroxypolydimethylsiloxane with a viscosity of 10000mPa·s at 25°C, 40 parts of dimethyl silicone oil with a viscosity of 100mPa·s, 100 parts of active nano calcium carbonate, and 10 parts of heavy calcium carbonate into a high-speed disperser, stir at normal pressure for 30 minutes, then evacuate and stir for 60 minutes at a temperature of 80-90°C and a vacuum degree of -0.08-0.099MPa, and cool to obtain.

[0040] Step 2: Preparation of component B: Specific surface area of ​​150m 2 / g of hydrophobic silica was heated in an oven at 105°C for 24h.

[0041] S1. Preparation of color paste: 100 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 20,000 mPa·s at 25°C, 30 parts of dimethyl silicone oil with a viscosity of 100 mPa·s, 10 parts of color pigment (medium chrome yellow, carbon black, iron red in a mass ratio of 1:1:1), and a specific surface area of ​​150 m 2 / g of hydrophobic white carbon black 30 parts, stir evenly, add 1 part of isocyanate methyl trimethoxy silane, stir thoroughly for 1 hour, heat to 120 ° C, dehydrate for 2 hours, cool and set aside;

[0042] S2, silicone rubber two-component vulcanizer and accelerator are pretreated and cooled to room temperature (25°C), sealed and stored for later use;

[0043] S3. Preparation of component B: put the above-obtained color paste, pre-treated silicone rubber two-component vulcanizer and accelerator, and 1 part of catalyst into a high-speed disperser, and stir evenly at room temperature and a vacuum degree of 0.08-0.099 MPa to obtain component B.

[0044] Step 3: Preparation of sealant: When using, mix the above-mentioned component A and component B in a mass ratio of 13:1 and cure in an environment with a temperature of 23°C and a humidity of 50%.

[0045] Example 2

[0046] A method for preparing a color-adjustable and storage-resistant two-component silicone structural sealant comprises the following steps:

[0047] Step 1, prepare component A: put 100 parts of α, ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s at 25°C, 30 parts of dimethyl silicone oil with a viscosity of 100 mPa·s, 80 parts of active nano calcium carbonate, and 30 parts of heavy calcium carbonate into a high-speed disperser, stir at normal pressure for 30 minutes, then evacuate and stir for 60 minutes at a temperature of 80-90°C and a vacuum degree of -0.08-0.099 MPa, and cool to obtain.

[0048] Step 2: Preparation of component B: Specific surface area of ​​150m 2 / g of hydrophobic silica was heated in an oven at 105°C for 24h.

[0049] S1. Preparation of color paste: 100 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 1500 mPa·s at 25°C, 60 parts of dimethyl silicone oil with a viscosity of 350 mPa·s, and 30 parts of color pigment with a specific surface area of ​​150 m 2 / g of hydrophobic white carbon black 50 parts, stir evenly, add 2 parts of isocyanate methyl trimethoxy silane, stir thoroughly for 1 hour, heat to 120 ° C, dehydrate for 2 hours, cool and set aside;

[0050] S2. Pretreatment of silicone rubber two-component vulcanizer and accelerator: Mix 80 parts of silicone rubber two-component vulcanizer and 1 part of zinc octanoate, stir them thoroughly for 2 hours at 40-60°C, then cool to room temperature (25°C), seal and store for later use;

[0051] S3. Preparation of component B: put the above-obtained color paste, the pre-treated silicone rubber two-component vulcanizer and accelerator, and 2 parts of the catalyst into a high-speed disperser, and stir evenly at room temperature and a vacuum degree of 0.08-0.099 MPa to obtain component B.

[0052] Step 3: Preparation of sealant: When using, mix the above-mentioned component A and component B in a mass ratio of 13:1, and cure in an environment with a temperature of 23°C and a humidity of 50%.

[0053] Example 3

[0054] A method for preparing a color-adjustable and storage-resistant two-component silicone structural sealant comprises the following steps:

[0055] Step 1, prepare component A: put 100 parts of α,ω-dihydroxypolydimethylsiloxane with a viscosity of 10000mPa·s at 25°C, 40 parts of dimethyl silicone oil with a viscosity of 350mPa·s, 80 parts of active nano calcium carbonate, and 20 parts of heavy calcium carbonate into a high-speed disperser, stir at normal pressure for 30 minutes, then evacuate and stir for 60 minutes at a temperature of 80-90°C and a vacuum degree of -0.08-0.099MPa, and cool to obtain.

[0056] Step 2: Preparation of component B: Specific surface area of ​​150m 2 / g of hydrophobic silica was heated in an oven at 105°C for 24h.

[0057] S1. Preparation of color paste: 100 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 20,000 mPa·s at 25°C, 30 parts of dimethyl silicone oil with a viscosity of 350 mPa·s, and 30 parts of color pigment with a specific surface area of ​​150 m 2 / g of hydrophobic white carbon black 30 parts, stir evenly, add 2 parts of isocyanate methyl trimethoxy silane, stir thoroughly for 1 hour, heat to 120 ° C, dehydrate for 2 hours, cool and set aside;

[0058] S2. Pretreatment of silicone rubber two-component vulcanizer and accelerator: Mix 60 parts of silicone rubber two-component vulcanizer and 1 part of sodium 2-ethylhexanoate, stir them thoroughly at 40-60°C for 2h, then cool to room temperature (25°C), seal and store for later use;

[0059] S3. Preparation of component B: put the above-obtained color paste, the pre-treated silicone rubber two-component vulcanizer and accelerator, and 2 parts of the catalyst into a high-speed disperser, and stir evenly at room temperature and a vacuum degree of 0.08-0.099 MPa to obtain component B.

[0060] Step 3: Preparation of sealant: When using, mix the above-mentioned component A and component B in a mass ratio of 15:1 and cure in an environment with a temperature of 23°C and a humidity of 50%.

[0061] Example 4

[0062] A method for preparing a color-adjustable and storage-resistant two-component silicone structural sealant comprises the following steps:

[0063] Step 1, prepare component A: put 100 parts of α, ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s at 25°C, 40 parts of dimethyl silicone oil with a viscosity of 350 mPa·s, 80 parts of active nano calcium carbonate, and 10 parts of heavy calcium carbonate into a high-speed disperser, stir at normal pressure for 30 minutes, then evacuate and stir for 60 minutes at a temperature of 80-90°C and a vacuum degree of -0.08-0.099 MPa, and cool to obtain.

[0064] Step 2: Preparation of component B: Specific surface area of ​​150m 2 / g of hydrophobic silica was heated in an oven at 105°C for 24h.

[0065] S1. Preparation of color paste: 100 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 1500 mPa·s at 25°C, 30 parts of dimethyl silicone oil with a viscosity of 100 mPa·s, and 30 parts of color pigment with a specific surface area of ​​150 m 2 / g of hydrophobic white carbon black 50 parts, stir evenly, add 1 part of isocyanate methyl trimethoxy silane, stir thoroughly for 1 hour, heat to 120 ° C, dehydrate for 2 hours, cool and set aside;

[0066] S2. Pretreatment of silicone rubber two-component vulcanizer and accelerator: Mix 80 parts of silicone rubber two-component vulcanizer and 1 part of sodium 2-ethylhexanoate, stir them thoroughly at 40-60°C for 2h, then cool to room temperature (25°C), seal and store for later use;

[0067] S3. Preparation of component B: put the above-obtained color paste, the pre-treated silicone rubber two-component vulcanizer and accelerator, and 2 parts of the catalyst into a high-speed disperser, and stir evenly at room temperature and a vacuum degree of 0.08-0.099 MPa to obtain component B.

[0068] Step 3: Preparation of sealant: When using, mix the above-mentioned component A and component B in a mass ratio of 15:1 and cure in an environment with a temperature of 23°C and a humidity of 50%.

[0069] Comparative Example 1

[0070] A method for preparing a color-adjustable and storage-resistant two-component silicone structural sealant comprises the following steps:

[0071] Step 1, prepare component A: put 100 parts of α, ω-dihydroxy polydimethylsiloxane with a viscosity of 10000 mPa·s at 25°C, 20 parts of dimethyl silicone oil with a viscosity of 100 mPa·s, 100 parts of active nano calcium carbonate, and 10 parts of heavy calcium carbonate into a high-speed disperser, stir at normal pressure for 30 minutes, then evacuate and stir for 60 minutes at a temperature of 80-90°C and a vacuum degree of -0.08-0.099 MPa, and cool to obtain.

[0072] Step 2: Preparation of component B: Specific surface area of ​​150m 2 / g of hydrophobic silica was heated in an oven at 105°C for 24h.

[0073] S1. Preparation of color paste: 100 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 20,000 mPa·s at 25°C, 60 parts of dimethyl silicone oil with a viscosity of 100 mPa·s and a specific surface area of ​​150 m 2 / g of hydrophobic white carbon black 50 parts, stir evenly, add 1 part of isocyanate methyl trimethoxy silane, stir thoroughly for 1 hour, heat to 120 ° C, dehydrate for 2 hours, cool and set aside;

[0074] S2. Pretreatment of silicone rubber two-component vulcanizer and accelerator: Mix 60 parts of silicone rubber two-component vulcanizer and 1 part of sodium 2-ethylhexanoate, stir them thoroughly at 40-60°C for 2h, then cool to room temperature (25°C), seal and store for later use;

[0075] S3. Preparation of component B: put the above-obtained color paste, pre-treated silicone rubber two-component vulcanizer and accelerator, and 1 part of catalyst into a high-speed disperser, and stir evenly at room temperature and a vacuum degree of 0.08-0.099 MPa to obtain component B.

[0076] Step 3: Preparation of sealant: When using, mix the above-mentioned component A and component B in a mass ratio of 15:1 and cure in an environment with a temperature of 23°C and a humidity of 50%.

[0077] Comparative Example 2

[0078] The difference between this comparative example and Example 1 is that when preparing component B, no stabilizer is added when preparing the color paste in step S1, and the other steps are exactly the same as in Example 1.

[0079] Comparative Example 3

[0080] The difference between this comparative example and Example 1 is that: when preparing component B, the silicone rubber two-component vulcanizing agent and accelerator in step S2 are not pretreated, and the other steps are exactly the same as in Example 1.

[0081] Comparative Example 4

[0082] The difference between this comparative example and Example 1 is that: when preparing component B, no stabilizer is added when preparing the color paste in step S1, and the two-component vulcanizer and accelerator of silicone rubber in step S2 are not pretreated. The other steps are exactly the same as in Example 1.

[0083] Comparative Example 5

[0084] The difference between this comparative example and Example 1 is that when preparing component B, a specific surface area of ​​150 m 2 / g of hydrophilic silica was heated in an oven at 105°C for 24h, and the other steps were exactly the same as in Example 1.

[0085] Comparative Example 6

[0086] The difference between this comparative example and Example 1 is that when preparing component B, when preparing the color paste in step S1, α,ω-dihydroxypolydimethylsiloxane with a viscosity of 20000 mPa·s at 25°C is used, and the other steps are exactly the same as in Example 1.

[0087] Experimental Example Performance Test

[0088] The components A and B in the examples and comparative examples were stored at a temperature of 23° C. and a humidity of 50% for 1 month and 6 months, and the sealant was prepared in step 3 at the expiration of the two periods, and the viscosity, curing time and mechanical properties of the sealant were tested.

[0089] 1. Viscosity test:

[0090] Test instrument: Bolefei DVPLUS

[0091] Test setting data: SC4-14, 100rpm, 30s

[0092] 2. Curing time test:

[0093] Test method: Test according to Appendix D of GB 16776-2005.

[0094] 3. Tensile bond strength test:

[0095] An H-shaped sample with one side being float glass (50mm*50mm) and the other side being anodized aluminum (50mm*50mm) was made, cured for 14 days in an environment of a temperature of 23°C and a humidity of 50%, and tested in accordance with the standard GB 16776-2005.

[0096] Table 1: Test results of Examples 1 to 4

[0097]

[0098]

[0099] Table 2: Comparative Examples 1 to 6 Related Test Results

[0100]

[0101] It can be seen from Examples 1 to 4 of the present invention and Comparative Examples 1 to 6 that, under the current formula and process, by adding a stabilizer, hydrophobic white carbon black, polyalkoxy-terminated polydimethylsiloxane, a vulcanizing agent and an accelerator for pretreatment, the prepared component B has excellent storage stability, which can reach more than 6 months compared to the comparative example, without thickening, and at the same time, the mechanical properties are stable, meeting the market sales and use requirements.

[0102] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A color-adjustable and storage-resistant two-component silicone structural sealant. Features: The invention comprises component A and component B, wherein the mass ratio of component A to component B is 13-15:1; component A comprises the following raw materials in mass ratio: 100 parts of α,ω-dihydroxy polydimethylsiloxane, 20-40 parts of dimethyl silicone oil, 80-100 parts of active nano calcium carbonate and 10-30 parts of heavy calcium carbonate; component B comprises the following raw materials in mass ratio: 100 parts of polyalkoxy-terminated polydimethylsiloxane, 30-60 parts of dimethyl silicone oil, 10-30 parts of color pigment, 30-50 parts of hydrophobic white carbon black, 60-80 parts of silicone rubber two-component vulcanizer, 1-2 parts of stabilizer, 0.5-1 part of accelerator and 1-2 parts of catalyst.

2. A color-adjustable, storage-resistant two-component silicone structural sealant according to claim 1, Features: The viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25°C is 10000-50000 mPa·s; the viscosity of the dimethyl silicone oil at 25°C is 100-350 mPa·s.

3. A color-adjustable and storage-resistant two-component silicone structural sealant according to claim 2, Features: The particle size of the active nano calcium carbonate is 800-1200 meshes; the particle size of the heavy calcium carbonate is 100-200 meshes.

4. A color-adjustable, storage-resistant two-component silicone structural sealant according to claim 3, Features: The viscosity of the polyalkoxy-terminated polydimethylsiloxane at 25° C. is 1500 to 20000 mPa·s; the specific surface area of ​​the hydrophobic white carbon black is 150 to 200 m 2 / g.

5. A color-adjustable, storage-resistant two-component silicone structural sealant according to claim 4, Features: The silicone rubber two-component vulcanizing agent is composed of at least two of ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, and phenyltriethoxysilane, and at least two of dimethyldimethoxysilane, diethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)γ-aminopropyltrimethoxysilane, and N-β-(aminoethyl)γ-aminopropyltriethoxysilane.

6. A color-adjustable, storage-resistant two-component silicone structural sealant according to claim 5, Features: The catalyst is one of dibutyltin dilaurate, dioctyltin dilaurate and dibutyltin acetate; the promoter is one of sodium isooctanoate, zinc isooctanoate and lithium isooctanoate.

7. A color-adjustable, storage-resistant two-component silicone structural sealant according to claim 6, Features: The stabilizer is isocyanate methyl trimethoxy silane.

8. The color-adjustable and storage-resistant two-component silicone structural sealant according to claim 7, Features: The coloring pigment is composed of at least three of medium chrome yellow, scarlet, iron red, brilliant red, carbon black, phthalocyanine blue, phthalocyanine green and titanium white.

9. A method for preparing a color-adjustable, storage-resistant two-component silicone structural sealant according to any one of claims 1 to 8, It is characterized in that The steps include: Step 1, preparing component A: stirring α,ω-dihydroxy polydimethylsiloxane, dimethyl silicone oil, active nano calcium carbonate and heavy calcium carbonate evenly; Step 2: Preparation of component B: S1. Preparation of color paste: polyalkoxy-terminated polydimethylsiloxane, dimethyl silicone oil, and color pigment are stirred evenly, and then isocyanate methyl trimethoxy silane is added. After sufficient stirring, the mixture is heated, dehydrated, and cooled for use; S2. Pretreatment of the two-component vulcanizer and accelerator of silicone rubber: after the two-component vulcanizer and accelerator of silicone rubber are mixed, heated and stirred, and then cooled; S3. Preparation of component B: Mix the color paste, the pre-treated silicone rubber two-component vulcanizer and accelerator, and the catalyst evenly to obtain component B. Step 3. Preparation of sealant: When using, mix component A and component B at a mass ratio of 13 to 15:1, degas, and cure at room temperature.

10. A color-adjustable, storage-resistant two-component silicone structural sealant and a preparation method thereof according to claim 9, Features: In step 1, the stirring conditions are: first stir at normal pressure for 30 minutes, then stir under vacuum for 60 minutes at a temperature of 80 to 90°C and a vacuum degree of -0.08 to 0.099 MPa, and then cool to obtain the product; in step 2, the heating temperature of S2 is 40 to 60°C, and the stirring time is 2 hours; in S3, the stirring conditions are room temperature and a vacuum degree of -0.08 to 0.099 MPa.