Mildew-proof, flame-retardant, antioxidant and tough soybean protein adhesive as well as preparation method and application thereof

Through the multi-crosslinked fiber reinforcement system of hydrogen bonds, covalent bonds and metal ion chelating bonds, the bonding strength and water resistance of soy protein adhesives are solved, mold resistance and flame retardancy are improved, and high performance is achieved bio-based adhesive.

CN118931491AActive Publication Date: 2024-11-12NANJING TECH UNIV

Patent Information

Application Number
CN202411254333.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing soy protein adhesives have problems such as low bonding strength, poor toughness of the glue layer, low initial viscosity, weak water resistance, poor mildew resistance, poor antibacteriality, low flame retardancy and poor oxidation resistance, which limits their use in artificial boards. Application in.

Method used

Using hydrogen bonds, covalent bonds and metal ion chelating bonds multiple crosslinked fiber reinforcement system, the hydroglycerol functionalization of seaweed nanofibers and soy proteins form a covalent crosslinking network, and the iron ions are introduced to improve the flame retardant properties of the adhesive. and toughness, and use the catechol groups of gallic acid to enhance anti-mold and anti-oxidant properties.

Benefits of technology

Significantly improves the bonding strength, water resistance, mildew resistance, antibacteriality and flame retardancy of soy protein adhesives, extends the service life of the adhesive, meets the national standards for artificial boards, and does not require expensive cross-linking. agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931491A_ABST
    Figure CN118931491A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, in particular to a mildewproof, flame-retardant, antioxidant and tough soybean protein adhesive as well as a preparation method and application thereof. The soybean protein adhesive comprises the following raw material components: soybean protein, water, a nano reinforcing agent and a modifier, the nano reinforcing agent is obtained by performing surface functionalization modification on seaweed nanofibers by gallic acid; the modifier is a metal ion compound. A gallic acid interface platform, the seaweed nanofibers and the soybean protein form a fiber-reinforced covalent bond and hydrogen bond cross-linked network, and metal ions and other components form sacrificial chelating bonds in the adhesive, so that a stable multi-cross-linked fiber-reinforced bionic hierarchical structure is constructed; the bonding strength, toughness, initial viscosity and water resistance of the adhesive are improved; in addition, the adhesive also has excellent mildew resistance, antibacterial property, flame retardance and oxidation resistance, and the process is simple to operate and easy to popularize and apply.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive modified by a functionalized nanofiber reinforcing agent and metal ions, and a preparation method and application thereof. Background Art

[0002] Adhesives are an important component of wood-based panels. Petroleum-based formaldehyde adhesives account for more than 90% of the market share of wood-based panel adhesives. However, petroleum-based formaldehyde adhesives have caused a series of environmental problems such as over-dependence on petrochemical resources and formaldehyde release. The development of high-performance, renewable, and environmentally friendly bio-based adhesives to replace petroleum-based formaldehyde adhesives is of great significance to solving the problems of petrochemical resource depletion and formaldehyde pollution.

[0003] As one of the most representative bio-based adhesives, soy protein adhesives have attracted extensive attention due to their easy availability, low price and good biocompatibility. However, poor bonding strength, adhesive toughness, initial adhesion and water resistance limit their practical applications.

[0004] In addition, the flammability of soy protein adhesives can lead to potentially fatal fire risks; at the same time, soy protein is susceptible to bacteria and mold, which seriously shortens the shelf life of the adhesive; in addition, soy protein adhesives are prone to adhesive failure after oxidation. Therefore, the development of strong soy protein adhesives with good water resistance, flame retardancy, mildew resistance, antibacterial and antioxidant properties is crucial for the development of wood adhesives.

[0005] Many materials in nature exhibit excellent strength and toughness at the same time, especially mussel byssus, which has a tensile strength of more than 100MPa; at the same time, the tensile fracture deformation exceeds 100%. The excellent mechanical properties of mussel byssus mainly come from the ordered hierarchical structure composed of a fiber core surrounded by a protective cuticle. The cuticle contains many particles and stores a large amount of catechol derivatives dopamine and iron ions. Iron ions and dopamine form coordination bonds, and dopamine self-polymerizes to form covalent bonds and hydrogen bonds for polydopamine. The internal fiber core provides structural stability, and the covalent bonds in the particles further strengthen the stability of the mussel byssus; on the other hand, the coordination bonds and hydrogen bonds act as sacrificial bonds to disperse the fracture energy, resulting in huge fracture toughness.

[0006] Seaweed nanofibers have excellent mechanical properties, are green and environmentally friendly, and are non-toxic, and have great potential for preparing high-performance composite materials. However, the chemical inertness of the surface of seaweed nanofibers leads to poor interfacial bonding with the matrix. Mussel-inspired catechol chemical modification is widely used to improve the surface reactivity of materials. The phenolic hydroxyl groups of catechol derivatives such as dopamine and gallic acid can be oxidized to quinones, which then react with nucleophiles to undergo Schiff base or Michael addition reactions, and at the same time undergo free radical coupling with other catechols or amines. Therefore, using catechol groups to improve the interfacial interaction between seaweed nanofibers and the matrix is ​​an effective design. Seaweed nanofibers with catechol groups can also serve as catechol donors to construct catechol-metal ion multi-crosslinked fiber-reinforced biomimetic hierarchical structures. Summary of the invention

[0007] Purpose of the invention: The technical problem to be solved by the present invention is to provide a nano-enhancer and a preparation method thereof, as well as a mildew-proof, flame-retardant, antioxidant and tough soybean protein adhesive prepared thereby, and a preparation method and application thereof.

[0008] Invention idea: Soy protein adhesive is modified by using hydrogen bond, covalent bond and metal ion chelate bond multiple cross-linked fiber reinforcement system, inspired by the hierarchical structure of catechol-iron ion multiple cross-linked fiber reinforcement in mussel byssus, using seaweed nanofibers to replace the byssus core, plant-derived gallic acid to replace dopamine in the byssus cuticle, ferric chloride to replace iron ions in the byssus cuticle, and soy protein to replace the protein matrix in the byssus cuticle, to construct a multiple cross-linked fiber reinforced bionic hierarchical structure. Gallic acid is used as a functionalized interface platform to graft seaweed nanofibers, which improves the reactivity and interface interaction between seaweed nanofibers and soy protein matrix. Functionalized seaweed nanofibers, as a reinforcing agent, form hydrogen bonds and covalent bonds with soy protein as well as a fiber reinforcement structure. The introduced iron ions, as a modifier, form metal ion chelate bonds with other components in the adhesive. The stable fiber-reinforced covalent cross-linked network improves the strength and water resistance of the adhesive, the sacrificial chelate bonds and hydrogen bonds improve the toughness of the adhesive, the hydrogen bonds and coordination effects increase the viscosity of the adhesive to increase the initial viscosity of the adhesive, the introduced gallic acid enhances the mildew resistance, antibacterial and antioxidant properties of the adhesive, the inorganic iron ions enhance the flame retardancy of the adhesive, and based on the multiple cross-linked bionic hierarchical structure, a mildew-resistant, flame-retardant, antioxidant and tough soy protein adhesive is prepared, which meets national standards in the application of artificial boards.

[0009] In order to solve the above technical problems, the present invention discloses the following technical solutions:

[0010] In a first aspect, the present invention provides a nano-enhancer, which is prepared by surface functionalization modification of seaweed nanofibers using gallic acid as a template.

[0011] Preferably, the nano-enhancer is made of raw materials including the following parts by weight: 285-315 parts of water, 3.6-10.4 parts of seaweed nanofibers, and 1.8-2.4 parts of gallic acid; preferably 290-310 parts of water, 3.8-9.2 parts of seaweed nanofibers, and 1.9-2.2 parts of gallic acid; preferably 300 parts of water, 4-8 parts of seaweed nanofibers, and 2 parts of gallic acid; the water is preferably deionized water.

[0012] Seaweed reserves are abundant in nature and are cheap. Using seaweed nanofibers to prepare high-performance composite materials not only achieves high-value utilization of seaweed, but also reduces seawater eutrophication and ecological damage caused by seaweed infestation. In addition, seaweed fibers themselves have strong rigidity and can serve as a skeleton core to increase the stability of the material.

[0013] Preferably, the seaweed nanofibers are obtained by treating natural seaweed with alkali to remove impurities and then acid hydrolyzing; preferably, the natural seaweed is added to a NaOH aqueous solution, stirred, washed and dried, and then added to sulfuric acid, stirred and washed; preferably, 10-15g of natural seaweed is added to 200-240mL of a 5-8wt% NaOH aqueous solution, stirred at 21-27°C for 24-28h, washed and dried to obtain 5-8g of alkali-treated seaweed, 5-7g of the obtained seaweed is added to 300-370mL of 55-60wt% sulfuric acid, stirred at 21-27°C for 12-17h, washed and dried to obtain 2.4-3.6g of the seaweed nanofibers; preferably, alkali treatment is first performed to remove impurities, 10-15g of natural seaweed is added to 200-240mL NaOH aqueous solution (5-8wt%), continuously stirred at a speed of 500-900r / min for 24-28h at a temperature of 21-27°C, repeatedly washed with water 3-7 times, and vacuum dried to obtain 5-8g of alkali-treated seaweed; then acid hydrolyzed, 5-7g of the alkali-treated seaweed was added to 300-370mL sulfuric acid (55-60wt%), continuously stirred at a speed of 800-1200r / min for 12-17h at a temperature of 21-27°C, and repeatedly washed with water 5-8 times, further preferably, the length of the seaweed nanofiber is 500-750nm, the width is 30-62nm, and 2.4-3.6g of seaweed nanofiber is obtained after vacuum drying; preferably, the weight of natural seaweed in the alkali treatment is 10-12g, the volume of the NaOH aqueous solution is 200-220mL, the concentration of the NaOH aqueous solution is 5-6wt%, stirred The temperature is 22-25°C, the stirring speed is 500-800r / min, the stirring time is 24-26h, the water is preferably deionized water, and the washing times are 3-5 times; the weight of the pretreated seaweed in the acid hydrolysis is 5-6g, the volume of sulfuric acid is 300-335mL, the concentration of sulfuric acid is 55-58wt%, the stirring temperature is 22-25°C, the stirring speed is 800-1000r / min, the stirring time is 12-14h, the water is preferably deionized water, and the washing times are 5-7 times; preferably, the length of the seaweed nanofiber is 500-630nm and the width is 30-47nm; the natural seaweed can be any one or a combination of Sargassum, Fucus, Dulse, Porphyra, and Gelidium; preferably, the natural seaweed is preferably Sargassum, and the present invention has been found through research that when the above-mentioned Sargassum is used, the comprehensive performance of the prepared seaweed nanofiber, especially the tensile strength, is better.

[0014] In some embodiments of the present invention, the gallic acid functionalized seaweed nanofiber raw material further includes a pH buffer regulator, such as Tris buffer solution.

[0015] The principle of gallic acid functionalized seaweed nanofibers in the present invention is that gallic acid has a catechol structure similar to dopamine, and can be adsorbed and grafted onto the surface of seaweed nanofibers through intermolecular hydrogen bonds and electrostatic interactions, providing more reactive sites for the seaweed nanofibers and increasing the interaction with the matrix.

[0016] In a second aspect, the present invention provides a method for preparing the nano-enhancer described in the first aspect, using gallic acid to functionalize the surface of seaweed nanofibers, comprising: mixing the seaweed nanofibers and water in parts by weight to obtain a seaweed nanofiber suspension, adjusting the pH to 7.0-8.5, then adding gallic acid, stirring continuously for 5.6-7.8 hours, repeatedly washing with water, and vacuum drying to obtain gallic acid-functionalized seaweed nanofibers.

[0017] Further, specifically, the seaweed nanofibers are added to water (preferably deionized water) according to a predetermined weight ratio and mixed evenly, a Tris buffer solution (1-1.8M) is used to adjust the pH to 7.5-8, and then gallic acid is added according to a specific amount, and the mixture is continuously stirred at a speed of 600-1000 r / min at a temperature of 23-29° C. for 6.1-7.3 hours. The mixture is washed with water for 3-5 times and vacuum dried to obtain 3.3-8.4 g of gallic acid functionalized seaweed nanofibers.

[0018] Preferably, the Tris buffer solution is 1-1.4M, the pH is adjusted to 7.8-8.2, the stirring temperature is 25-27°C, the stirring speed is 600-800r / min, the stirring time is 6.7-7.1h, the water is preferably deionized water, the washing times are 3-4 times, and 3.6-7.8g of gallic acid functionalized seaweed nanofibers are obtained.

[0019] The present invention has been found through research that the uniformity, dispersibility and enhancement effect of the nano-enhancer prepared by using the above-mentioned optimized process parameters are better.

[0020] In the third aspect, the present invention also provides a modified soy protein adhesive, comprising the above-mentioned gallic acid functionalized seaweed nanofibers, utilizing gallic acid functionalized seaweed nanofibers as fiber cores and catechol donors, and adding metal ions to construct a mussel byssus structure, thereby solving the problems of low bonding strength of the adhesive, poor toughness of the adhesive layer, low initial adhesion, weak water resistance, poor mildew resistance, poor antibacterial property, low flame retardancy and poor antioxidant property.

[0021] The invention is subjected to catechol-Fe in mussel byssus 3+ Inspired by the multi-crosslinked fiber-reinforced hierarchical structure, seaweed nanofibers are used to simulate the fiber core in mussel byssus, gallic acid simulates dopamine in byssus, and metal ions simulate Fe in byssus 3+, soybean protein simulates the protein matrix in the byssus, thereby preparing a mildew-proof, flame-retardant, antioxidant and tough soybean protein adhesive based on the structure of mussel byssus. Seaweed nanofibers are covalently cross-linked with soybean protein molecules through the gallic acid interfacial reaction activity platform to construct a covalent cross-linked network. At the same time, the catechol groups of gallic acid form hydrogen bonds with the interface of the wood substrate and the adhesive forms glue nails, which increases the cohesion of the adhesive, the adhesion to the interface of the substrate and the internal cross-linking hydrophobic stability, thereby improving the bonding strength and water resistance; metal ions form chelate bonds with the functionalized seaweed nanofibers and soybean proteins. During the stretching process, the chelate bonds can act as sacrificial bonds to dissipate energy, thereby improving the toughness of the adhesive layer; the hydrogen bonds and chelate bonds formed improve the shear resistance of the adhesive , thereby increasing the viscosity and improving the initial viscosity of the adhesive; the catechol group of gallic acid can adhere to fungal cells and change the permeability of fungal cell membranes, killing fungi, thereby improving the mildew resistance and antibacterial properties of the adhesive; the phenolic hydroxyl group of gallic acid, especially the ortho-hydroxyl group, exerts a strong antioxidant effect through the transfer of hydrogen atoms and single electrons, thereby improving the antioxidant properties of the adhesive; inorganic metal ions promote the dehydration and carbonization of soy protein molecules during combustion to form a char layer. The char layer acts as a physical fire barrier, hindering the penetration of external oxygen and delaying the decomposition of the internal combustible matrix, thereby improving the flame retardancy of the adhesive.

[0022] More specifically, the modified soybean protein adhesive provided by the present invention comprises soybean protein, water, a reinforcing agent and a modifier.

[0023] Furthermore, the modified soy protein adhesive comprises the following raw material components in parts by weight: 2-7 parts of soy protein, 14-25 parts of water, 0.4-1.2 parts of nano-enhancer, and 0.2-0.8 parts of modifier; preferably, the raw material components of the modified soy protein adhesive include, in parts by weight: 2.5-5 parts of soy protein, 16-21 parts of water, 0.6-1.0 parts of nano-enhancer, and 0.4-0.6 parts of modifier; preferably, the raw material components of the modified soy protein adhesive include, in parts by weight: 3 parts of soy protein, 17 parts of water, 0.6-1.0 parts of nano-enhancer, and 0.4-0.6 parts of modifier.

[0024] Preferably, the modifier is a metal ion, which may be Fe 3+ 、Al 3+ Cr 3+ Preferably, the modifier is Fe 3+ (Preferably FeCl3), the present invention has found through research that when the above-mentioned FeCl3 is used, the comprehensive performance of the adhesive, especially the bonding strength, adhesive layer toughness and flame retardancy is better.

[0025] Preferably, the soy protein is soy protein isolate with a protein content of 91-98wt%, preferably 93-95wt%; a particle size of 150-350 mesh, preferably 220-260 mesh; it can be one or more of high-temperature soluble soy protein isolate, low-temperature soluble soy protein isolate, and defatted soy protein isolate; and the water is preferably deionized water.

[0026] In a fourth aspect, the present invention also provides a method for preparing the modified soy protein adhesive, comprising the steps of blending and uniformly stirring soy protein, water, a reinforcing agent and a modifier in predetermined weight proportions.

[0027] As preferred include:

[0028] 1) slowly adding soybean protein into water and blending with water, stirring at a constant rate for a first time, stirring evenly, to obtain soybean protein colloid; 2) slowly introducing the enhancer into the soybean protein colloid, stirring at a constant rate for a second time, stirring evenly, to obtain enhanced soybean protein colloid; 3) slowly introducing the modifier into the enhanced soybean protein colloid, stirring at a constant rate for a third time, stirring evenly, to obtain modified soybean protein colloid. Preferably, the first stirring is continuous stirring at a speed of 900-1900 r / min at a temperature of 25-35°C for 20-35 min; preferably, the second stirring is continuous stirring at a speed of 600-1400 r / min at a temperature of 25-33°C for 15-25 min; preferably, the third stirring is continuous stirring at a speed of 500-1200 r / min at a temperature of 25-30°C for 10-20 min; preferably, the nano-enhancer is added to the reaction system in 3-7 times, preferably with an interval of 1-4 min each time, and preferably the amount added each time is 1 / the total amount; preferably, the modifier is added to the reaction system in 1-3 times, preferably with an interval of 5-10 min each time, and preferably the amount added each time is 1 / the total amount.

[0029] As preferred include:

[0030] 1) Slowly add soybean protein into water and mix with water, and stir continuously for 20-35 minutes at a speed of 900-1900 r / min and a temperature of 25-35° C. to obtain soybean protein gelatin.

[0031] 2) The enhancer is slowly introduced into the above soybean protein colloid solution 3-7 times (1 / time of the total amount is added each time, and the interval between each addition is 3-6 minutes), and then stirred for 15-25 minutes at a speed of 600-1400 r / min and a temperature of 25-33° C. to obtain an enhanced soybean protein colloid solution.

[0032] 3) slowly introducing the modifier into the enhanced soybean protein colloid solution 1-3 times (1 / time of the total amount added each time, with an interval of 5-10 minutes each time), and then stirring at a speed of 500-1200 r / min at a temperature of 25-30° C. for 10-20 minutes to obtain a modified soybean protein colloid solution.

[0033] The present invention adopts the above method to facilitate the formation of catechol-Fe in bionic mussel byssus 3+ The hierarchical structure reinforced by multiple cross-linked fibers is conducive to better increasing the bonding strength, adhesive layer toughness, initial adhesion, water resistance, mildew resistance, antibacterial property, flame retardancy and antioxidant property of the modified soy protein adhesive.

[0034] More preferably, the preparation method of the modified soy protein adhesive specifically comprises:

[0035] 1) Slowly add soybean protein into water and mix with water, and stir continuously for 20-28 minutes at a speed of 1100-1600 r / min and a temperature of 25-31° C. to obtain soybean protein gelatin.

[0036] 2) The enhancer is slowly introduced into the above soybean protein colloid solution 3-5 times (1 / time of the total amount is added each time, and the interval between each addition is 3-5 minutes), and then the mixture is stirred at a speed of 900-1100 r / min and a temperature of 25-29° C. for 15-22 minutes to obtain an enhanced soybean protein colloid solution.

[0037] 3) slowly introducing the modifier into the enhanced soybean protein colloid solution 2-3 times (1 / time of the total amount added each time, 5-8 minutes interval between each addition), and then stirring for 12-18 minutes at a speed of 500-800 r / min and a temperature of 25-27° C. to obtain a modified soybean protein colloid solution.

[0038] Preferably, the water used in the above preparation process is deionized water.

[0039] The present invention has been found through research that the comprehensive properties of the modified adhesive prepared by using the above-mentioned optimized process parameters are better, especially the mechanical properties and water resistance.

[0040] In the fifth aspect, the present invention also provides the application of the modified soybean protein adhesive in formaldehyde-free artificial boards. The adhesive in the present invention is green and environmentally friendly, does not contain harmful ingredients such as formaldehyde, and has high performance and multi-functions, which can increase the applicability of the adhesive during the preparation of artificial boards. The prepared artificial boards meet the strength requirements. The high toughness of the adhesive layer prevents the edges from breaking and cracking when the artificial boards are sawed and shaped. The high viscosity and high initial viscosity of the adhesive can prevent the slabs from stratifying after assembly. The prepared artificial boards are still firm and will not debond when used in a humid environment. The prepared artificial boards have strong flame retardancy, which reduces the risk of fire. The adhesive layer of the prepared artificial boards is mildew-proof and antibacterial during use, which reduces the damage of mold and bacteria to the adhesive layer and improves the stability of the artificial boards. At the same time, the adhesive layer of the prepared artificial boards has strong antioxidant properties, which prevents the adhesive layer from failing due to oxidation, and can extend the service life of the artificial boards. Preferably, the above-mentioned artificial boards can be one or more of plywood, medium-density fiberboard, particleboard and blockboard.

[0041] In a sixth aspect, the present invention also provides a method for producing formaldehyde-free plywood using the modified soy protein adhesive, comprising: applying the adhesive on a wood veneer, and then assembling and hot pressing.

[0042] Preferably, the preparation process of plywood includes: 2 The modified soybean protein adhesive was applied on one side of a 400mm×400mm×1.6mm wood veneer using a glue roller, and the core layer veneer and the adjacent upper and bottom veneers were assembled and assembled in a vertical direction. Then, the assembled veneers were placed on a metal pad, and the assembled veneers were fixed with the metal pad, and then placed on a CGYJ-100 hot press, and the press parameters were adjusted to 1MPa pressure, 120℃ temperature, and 315s time for hot pressing.

[0043] Preferably, the wood veneer used can be one or more of poplar veneer, eucalyptus veneer, pine veneer and fir veneer; preferably, the moisture content of the wood veneer is controlled at 8-12%.

[0044] The technical solution provided by the present invention uses seaweed as a raw material for processing to obtain seaweed nanofibers, thereby achieving high-value utilization; at the same time, compared with macromolecular polyphenols, the present invention uses small-molecule gallic acid to hydrogen-bond the fiber surface, so that the fiber surface has carboxyl groups in addition to phenolic hydroxyl groups. The carboxyl groups will form a complex with soybean protein molecules, increase the stability of the cured structure, and increase the initial adhesion with the wood interface, so that the pre-pressing performance of the plywood is better, and the assembled slabs are prevented from being delaminated during transportation. The slabs are suitable for gluing high-moisture-content veneers into boards, and the processability in the actual manufacturing process of the artificial board is improved.

[0045] The beneficial effects of the present invention include:

[0046] 1) Based on the hierarchical and orderly structure of mussel byssus, the present invention proposes an effective bionic method to modify soybean protein adhesive, using seaweed nanofibers to imitate the fiber core in byssus, gallic acid to imitate dopamine in byssus, and metal ions to imitate Fe in byssus. 3+ , soy protein mimics the protein matrix in the byssus. Gallic acid as an interface platform improves the interaction between the reinforcing agent and soy protein. Gallic acid functionalized seaweed nanofibers and soy protein form a fiber-reinforced covalent and hydrogen bond cross-linked network. Metal ions form sacrificial chelate bonds with other components, thereby constructing a stable multiple cross-linked fiber-reinforced bionic hierarchical structure, solving the problems of low bonding strength, poor water resistance and poor toughness of the adhesive, so that the strength and water resistance meet the national standards, and the toughness of the adhesive layer meets the requirements of not easy to break; multiple bonds improve the viscosity and initial adhesion of the adhesive, so that the plywood after adhesive coating and assembly is not easy to delaminate, and prevent the plywood after assembly from being displaced during transportation; the catechol group of gallic acid destroys the membrane structure of fungi, prolongs the service life of the adhesive, and solves the problem of poor mildew resistance and antibacterial properties; the phenolic hydroxyl group of gallic acid gives the adhesive effective antioxidant properties, solving the problem of poor antioxidant properties; the inorganic hybrid system of metal ions promotes the formation of a fireproof carbonized layer in the adhesive layer, solving the problem of poor flame retardancy of the adhesive.

[0047] 2) The adhesive prepared by the present invention is green and pollution-free, does not produce harmful components such as formaldehyde, and does not cause harm to the environment and human health.

[0048] 3) The raw materials used in the adhesive of the present invention are sustainable, and no petroleum-based raw materials are used, thereby reducing the excessive use of non-renewable resources.

[0049] 4) The soybean protein and seaweed nanofibers in the present invention are both made from industrial food byproducts and natural waste, which reduces the waste of resources and is conducive to the high-value utilization of resources.

[0050] 5) The raw material cost of the adhesive in the present invention is low, and no other expensive additives and cross-linking agents need to be added, which is beneficial to improving social and economic benefits.

[0051] 6) The process of the present invention is easy to operate, does not require complicated machinery and equipment, and is conducive to practical industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0053] Figure 1It is a graph showing the dry bonding strength results of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention.

[0054] Figure 2 It is a graph showing the fracture toughness results of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention.

[0055] Figure 3 It is a graph showing the viscosity results of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention.

[0056] Figure 4 It is a graph showing the wet bonding strength results of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention.

[0057] Figure 5 It is a graph showing the anti-mildew validity period of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention.

[0058] Figure 6 It is a graph showing the antibacterial rate results of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention.

[0059] Figure 7 This is a graph showing the flame retardancy results of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention - Limiting Oxygen Index.

[0060] Figure 8 It is the flame retardancy result diagram of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention - Maximum heat release rate.

[0061] Fig. 9 This is the antioxidant result diagram of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention - absorbance.

[0062] Fig.10 This is a graph showing the antioxidant properties of the adhesives of Comparative Examples 1-6 and Examples 1-5 of the present invention - total antioxidant capacity. DETAILED DESCRIPTION

[0063] The experimental methods described in the present invention are all conventional methods unless otherwise specified.

[0064] The materials or reagents used in the present invention, if the manufacturer is not indicated, can be obtained through regular commercial channels.

[0065] In the present invention, soybean protein powder (protein content 95%, particle size 220-260 mesh) was purchased from Anhui Shuinuo Biotechnology Co., Ltd., seaweed was purchased from Guangdong Dianmei Biotechnology Co., Ltd., gallic acid was purchased from Shanghai Ciyu Chemical Technology Co., Ltd., and ferric chloride (FeCl3, 99%) was provided by Fujian Beiwan Reagent Co., Ltd.

[0066] The present invention provides a nano-enhancer (functionalized seaweed nanofiber) and a metal ion-modified mildew-proof, flame-retardant, antioxidant and tough soybean protein adhesive and a preparation method thereof. Specific embodiments are as follows.

[0067] Example 1

[0068] This embodiment provides a nano-enhancer and a mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and a preparation method thereof, as follows:

[0069] The preparation method of the nano-enhancer (functionalized seaweed nanofiber) in Example 1 is as follows:

[0070] 1) First, the natural Sargassum is subjected to alkali treatment, 10 g of the natural Sargassum is added to 200 mL of a NaOH aqueous solution (5 wt%), and the mixture is continuously stirred at 500 r / min for 24 h at 25° C., washed with water for 3 times to remove impurities, and dried in a vacuum; then, the seaweed is subjected to acid hydrolysis, 5 g of the alkali-treated seaweed is added to 300 mL of sulfuric acid (55 wt%), and the mixture is continuously stirred at 800 r / min for 12 h at 25° C., washed with water for 5 times to make the pH of the fiber neutral, and the seaweed nanofiber is further preferably 500-600 nm long and 30-45 nm wide, and 2.4-2.7 g of seaweed nanofiber is obtained after vacuum drying, and the preparation process is repeated to obtain sufficient seaweed nanofiber and store it at 5° C. for standby use.

[0071] 2) Add 4 g of seaweed nanofibers into 300 mL of deionized water and mix well to obtain a suspension. Use Tris buffer solution (1 M) to adjust the pH of the suspension to 8. Then, add 2 g of gallic acid to the suspension. Stir continuously for 7 h at a speed of 600 r / min at 25 ° C. Wash 3 times with deionized water and then vacuum dry to obtain 3.8 g of gallic acid-functionalized seaweed nanofibers.

[0072] The mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and its preparation method in Example 1 have the following raw material weight proportions:

[0073]

[0074] The preparation method of the above adhesive is as follows:

[0075] 1) First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein gelatin.

[0076] 2) Slowly add 0.6 parts of the prepared enhancer (functionalized seaweed nanofibers) into the above-mentioned soybean protein colloid solution in 3 times (1 / 3 of the total amount is added each time, and the interval between each time is 3 minutes), and then continue to stir at a speed of 1000 r / min at a temperature of 25°C for 20 minutes to obtain an enhanced soybean protein colloid solution.

[0077] 3) Slowly introduce 0.4 parts of the prepared modifier (FeCl3) into the above-mentioned enhanced soy protein colloid in 2 times (1 / 2 of the total amount is added each time, with an interval of 5 minutes each time), and then continue stirring at a speed of 800r / min at a temperature of 25°C for 15 minutes to obtain a modified soy protein colloid.

[0078] Example 2

[0079] This embodiment provides a nano-enhancer and a mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and a preparation method thereof, as follows:

[0080] The specific process of the preparation method of the nano-enhancer (functionalized seaweed nanofiber) in Example 2 is the same as the preparation method of the nano-enhancer in Example 1.

[0081] The mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and its preparation method in Example 2 have the following raw material weight proportions:

[0082]

[0083]

[0084] The preparation method of the above adhesive is as follows:

[0085] 1) First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein gelatin.

[0086] 2) Slowly add 0.8 parts of the prepared enhancer (functionalized seaweed nanofibers) into the above-mentioned soybean protein colloid solution in 4 times (1 / 4 of the total amount is added each time, with an interval of 3 minutes each time), and then continue stirring at a speed of 1000 r / min at a temperature of 25°C for 20 minutes to obtain an enhanced soybean protein colloid solution.

[0087] 3) Slowly introduce 0.4 parts of the prepared modifier (FeCl3) into the above-mentioned enhanced soy protein colloid in 2 times (1 / 2 of the total amount is added each time, with an interval of 5 minutes each time), and then continue stirring at a speed of 800r / min at a temperature of 25°C for 15 minutes to obtain a modified soy protein colloid.

[0088] Example 3

[0089] This embodiment provides a nano-enhancer and a mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and a preparation method thereof, as follows:

[0090] The specific process of the preparation method of the nano-enhancer (functionalized seaweed nanofiber) in Example 3 is the same as the preparation method of the nano-enhancer in Example 1.

[0091] The mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and its preparation method in Example 3 have the following raw material weight proportions:

[0092]

[0093] The preparation method of the above adhesive is as follows:

[0094] 1) First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein gelatin.

[0095] 2) 1.0 portion of the prepared reinforcing agent (functionalized seaweed nanofibers) was slowly added to the above soybean protein colloid solution in 5 times (1 / 5 of the total amount was added each time, with an interval of 3 minutes each time), and then stirred at a speed of 1000 r / min at a temperature of 25°C for 20 minutes to obtain a reinforced soybean protein colloid solution.

[0096] 3) Slowly introduce 0.4 parts of the prepared modifier (FeCl3) into the above-mentioned enhanced soy protein colloid in 2 times (1 / 2 of the total amount is added each time, with an interval of 5 minutes each time), and then continue stirring at a speed of 800r / min at a temperature of 25°C for 15 minutes to obtain a modified soy protein colloid.

[0097] Example 4

[0098] This embodiment provides a nano-enhancer and a mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and a preparation method thereof, as follows:

[0099] Different preparation methods were used to synthesize nano-enhancers (functionalized seaweed nanofibers). Different nano-enhancers were synthesized by changing the proportions. The specific process is as follows:

[0100] The specific process of the preparation method of the nano-enhancer in Example 4 is the same as the preparation method of the nano-enhancer in Example 1, except that: in this example 2) 6 g of seaweed nanofibers are added to 300 mL of deionized water and mixed evenly to obtain a suspension, and the pH of the suspension is adjusted to 8 using Tris buffer solution (1 M), and then 2 g of gallic acid is added to the suspension, and the suspension is continuously stirred at a speed of 600 r / min at a temperature of 25°C for 7 h, washed with deionized water 3 times, and then vacuum dried to obtain 5.4 g of gallic acid-functionalized seaweed nanofibers.

[0101] The mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and its preparation method in Example 4 have the following raw material weight proportions:

[0102]

[0103] The different nano-enhancers obtained in the above Example 4 were used to prepare mildew-proof, flame-retardant, antioxidant and tough soybean protein adhesives. The method for preparing the soybean protein adhesive was the same as that in Example 2.

[0104] Example 5

[0105] This embodiment provides a nano-enhancer and a mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and a preparation method thereof, as follows:

[0106] Different preparation methods were used to synthesize nano-enhancers (functionalized seaweed nanofibers). Different nano-enhancers were synthesized by changing the proportions. The specific process is as follows:

[0107] The specific process of the preparation method of the nano-enhancer in Example 5 is the same as the preparation method of the nano-enhancer in Example 1, except that: in this example 2) 8 g of seaweed nanofibers are added to 300 mL of deionized water and mixed evenly to obtain a suspension, and the pH of the suspension is adjusted to 8 using Tris buffer solution (1 M), and then 2 g of gallic acid is added to the suspension, and the suspension is continuously stirred at a speed of 600 r / min at a temperature of 25°C for 7 h, washed with deionized water 3 times, and then vacuum dried to obtain 7.2 g of gallic acid-functionalized seaweed nanofibers.

[0108] The mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and its preparation method in Example 5 have the following raw material weight proportions:

[0109]

[0110] The different nano-enhancers obtained in the above Example 5 were used to prepare mildew-proof, flame-retardant, antioxidant and tough soybean protein adhesives. The method for preparing the soybean protein adhesive was the same as that in Example 2.

[0111] Comparative Example 1

[0112] This comparative example provides a soybean protein adhesive and a preparation method thereof, as follows:

[0113] The soybean protein adhesive prepared in Comparative Example 1 is different from that in Example 2 in that no reinforcing agent (functionalized seaweed nanofibers) and no modifier (FeCl3) are added during the preparation process, and the rest are the same.

[0114] The soy protein adhesive and preparation method thereof in Comparative Example 1, the weight proportion of raw materials is as follows:

[0115] 3 servings of soy protein

[0116] 17 parts water

[0117] The preparation method of the above adhesive is as follows:

[0118] First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein colloid.

[0119] Comparative Example 2

[0120] This comparative example provides a nano-enhancer and a modified soybean protein adhesive and a preparation method thereof, as follows:

[0121] Ordinary seaweed nanofibers (unfunctionalized) were used as nanoreinforcement agents to prepare ordinary seaweed nanofibers. The specific process is as follows:

[0122] The specific process of the preparation method of the nano-enhancer in Comparative Example 2 is the same as that of the preparation method of the nano-enhancer in Example 2, except that: the preparation process of the nano-enhancer in this comparative example does not include step 2).

[0123] The soy protein adhesive prepared in Comparative Example 2 is different from that in Example 2 in that ordinary seaweed nanofibers (unfunctionalized) are used as nano-reinforcement agents to modify the soy protein adhesive, and no modifier (FeCl3) is added during the preparation process. The rest is the same.

[0124] The modified soybean protein adhesive and preparation method thereof in Comparative Example 2, the weight proportion of raw materials is as follows:

[0125] 3 servings of soy protein

[0126] 17 parts water

[0127] Enhancer 0.8 parts

[0128] The preparation method of the above adhesive is as follows:

[0129] 1) First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein gelatin.

[0130] 2) Slowly add 0.8 parts of the prepared enhancer (ordinary seaweed nanofiber) into the above-mentioned soybean protein colloid solution in 4 times (1 / 4 of the total amount is added each time, and the interval between each time is 3 minutes), and then continue to stir at a speed of 1000r / min at a temperature of 25°C for 20 minutes to obtain an enhanced soybean protein colloid solution.

[0131] Comparative Example 3

[0132] This comparative example provides a nano-enhancer and a modified soybean protein adhesive and a preparation method thereof, as follows:

[0133] The specific process of the preparation method of the nano-enhancer (functionalized seaweed nanofiber) in Comparative Example 3 is the same as that of the preparation method of the nano-enhancer in Example 2.

[0134] The soybean protein adhesive prepared in Comparative Example 3 is different from that in Example 2 in that no modifier (FeCl3) is added during the preparation process, and the rest is the same.

[0135] The modified soybean protein adhesive and preparation method thereof in Comparative Example 3, the weight proportion of raw materials is as follows:

[0136] 3 servings of soy protein

[0137] 17 parts water

[0138] Enhancer 0.8 parts

[0139] The preparation method of the above adhesive is as follows:

[0140] 1) First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein gelatin.

[0141] 2) Slowly add 0.8 parts of the prepared enhancer (functionalized seaweed nanofibers) into the above-mentioned soybean protein colloid solution in 4 times (1 / 4 of the total amount is added each time, with an interval of 3 minutes each time), and then continue stirring at a speed of 1000 r / min at a temperature of 25°C for 20 minutes to obtain an enhanced soybean protein colloid solution.

[0142] Comparative Example 4

[0143] This comparative example provides a soybean protein adhesive and a preparation method thereof, as follows:

[0144] The soybean protein adhesive prepared in Comparative Example 4 is different from that in Example 2 in that no reinforcing agent (functionalized seaweed nanofibers) is added during the preparation process, and the rest is the same.

[0145] The soy protein adhesive and preparation method thereof in Comparative Example 4, the weight proportion of raw materials is as follows:

[0146] 3 servings of soy protein

[0147] 17 parts water

[0148] Modifier 0.4 parts

[0149] The preparation method of the above adhesive is as follows:

[0150] 1) First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein gelatin.

[0151] 2) Slowly introduce 0.4 parts of the prepared modifier (FeCl3) into the above-mentioned enhanced soy protein colloid in 2 times (1 / 2 of the total amount is added each time, with an interval of 5 minutes each time), and then continue stirring at a speed of 800r / min at a temperature of 25°C for 15 minutes to obtain a modified soy protein colloid.

[0152] Comparative Example 5

[0153] This comparative example provides a nano-enhancer and a modified soybean protein adhesive and a preparation method thereof, as follows:

[0154] The specific process of the preparation method of the nano-enhancer (functionalized seaweed nanofiber) in Comparative Example 5 is the same as that of the preparation method of the nano-enhancer in Example 2.

[0155] The soybean protein adhesive prepared in Comparative Example 5 is different from that in Example 2 in that another modifier (AlCl3) is added during the preparation process, and the rest is the same.

[0156] The mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and its preparation method in Comparative Example 5 have the following raw material weight ratios:

[0157]

[0158] The preparation method of the above adhesive is as follows:

[0159] 1) First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein gelatin.

[0160] 2) Slowly add 0.8 parts of the prepared enhancer (functionalized seaweed nanofibers) into the above-mentioned soybean protein colloid solution in 4 times (1 / 4 of the total amount is added each time, with an interval of 3 minutes each time), and then continue stirring at a speed of 1000 r / min at a temperature of 25°C for 20 minutes to obtain an enhanced soybean protein colloid solution.

[0161] 3) Slowly introduce 0.4 parts of the prepared modifier (AlCl3) into the above-mentioned enhanced soybean protein colloid in 2 times (1 / 2 of the total amount is added each time, with an interval of 5 minutes each time), and then continue stirring at a speed of 800r / min at a temperature of 25°C for 15 minutes to obtain a modified soybean protein colloid.

[0162] Comparative Example 6

[0163] This comparative example provides a nano-enhancer and a modified soybean protein adhesive and a preparation method thereof, as follows:

[0164] The specific process of the preparation method of the nano-enhancer (functionalized seaweed nanofiber) in Comparative Example 6 is the same as that of the preparation method of the nano-enhancer in Example 2.

[0165] The soybean protein adhesive prepared in Comparative Example 6 is different from that in Example 2 in that another modifier (CrCl3) is added during the preparation process, and the rest is the same.

[0166] The mildew-proof, flame-retardant, anti-oxidation and tough soybean protein adhesive and its preparation method in Comparative Example 6 have the following raw material weight proportions:

[0167]

[0168] The preparation method of the above adhesive is as follows:

[0169] 1) First, 17 parts of water were added into a reactor equipped with a stirring function, and then 3 parts of soybean protein were slowly added into the reactor and mixed with water, and then stirred continuously at a speed of 1200 r / min at a temperature of 25° C. for 25 minutes to obtain soybean protein gelatin.

[0170] 2) Slowly add 0.8 parts of the prepared enhancer (functionalized seaweed nanofibers) into the above-mentioned soybean protein colloid solution in 4 times (1 / 4 of the total amount is added each time, with an interval of 3 minutes each time), and then continue stirring at a speed of 1000 r / min at a temperature of 25°C for 20 minutes to obtain an enhanced soybean protein colloid solution.

[0171] 3) Slowly introduce 0.4 parts of the prepared modifier (CrCl3) into the above-mentioned enhanced soy protein gum solution in 2 times (1 / 2 of the total amount is added each time, with an interval of 5 minutes each time), and then continue stirring at a speed of 800r / min at a temperature of 25°C for 15 minutes to obtain a modified soy protein gum solution.

[0172] Experimental Example 1

[0173] The soy protein adhesive obtained in the above Examples 1-5 and Comparative Examples 1-6 is used to prepare three-layer plywood. The specific preparation process and process are as follows:

[0174] Poplar veneer with a size of 400mm×400mm×1.6mm is used as the plywood substrate. The moisture content of the poplar veneer is controlled at 8%-12%. The moisture content is 180g / m 2 The modified soy protein adhesive is applied on one side of the veneer substrate using a glue roller. When assembling the three-layer plywood, the veneer of the core layer is arranged and assembled vertically with the veneers of the adjacent upper and bottom layers. The hot pressing parameters are set to a pressure of 1 MPa, a temperature of 120°C and a time of 315 s. After continuous hot pressing, the prepared three-layer plywood is taken out from the press.

[0175] Adhesive bonding performance, toughness and water resistance testing:

[0176] According to the test methods for physical and chemical properties of wood-based panels and veneer wood-based panels in GB / T 17657-2013, the dry bonding strength, fracture toughness and wet bonding strength of the plywood prepared with adhesives were tested. The fracture toughness reflects the toughness of the adhesive, and the wet bonding strength reflects the water resistance of the adhesive. The test results are shown in Figure 1 , Figure 2 , Figure 4 .

[0177] Adhesive viscosity test:

[0178] The viscosity of the adhesive was measured on a RST-CPS rheometer using a 20 mm diameter parallel plate fixture. During the measurement, the distance was set to 1 mm and the shear rate was set from 1-50 rad / s. The viscosity reflects the initial viscosity of the adhesive. The test results are shown in Figure 3 .

[0179] Adhesive anti-mildew performance test:

[0180] 15g of uncured adhesive was placed in a culture dish and stored at 30°C and 80% relative humidity. The mold and decomposition of the adhesive samples were then observed every day. The anti-mold validity period of the adhesive was recorded and counted in days. The test results are shown in Figure 5 .

[0181] Adhesive antibacterial performance test:

[0182] The antibacterial rate was determined by the colony counting method. The adhesive was first dried at 120°C to constant weight and ground into 200-mesh powder. The adhesive powder sample was mixed with sterile water to make a solution with a concentration of 20 mg / mL. The bacterial strain was activated after being cultured in an incubator at 37°C. The activated bacteria (0.5×10 5 CFU / mL) was placed in a PBS buffer (5mL) containing the above adhesive solution and cultured at 37°C for 4h. The bacterial solution obtained after culture was diluted 10 times, and 40μL of it was spread on Luria-Bertani (LB) agar medium. The number of colonies was counted after incubation at 37°C for 4h. The antibacterial rate of the adhesive was calculated as N2 / N1 and converted into a percentage, where N1 is the number of colonies not treated with the adhesive sample, and N2 is the number of colonies treated with the adhesive sample. The test results are shown in Figure 6 .

[0183] Adhesive flame retardant performance test:

[0184] The limiting oxygen index of the adhesive samples was measured using an oxygen index flammability tester (HC-2C) according to GB / T 5454-1997; the maximum heat release rate of the adhesive samples was tested on an FTT cone calorimeter according to ISO 5660-1, with a heat flux of 55kW / m 2 , the test results are shown in Figure 7 and Figure 8 .

[0185] Adhesive Antioxidant Performance Test:

[0186] The antioxidant activity of the adhesive was determined using the azo-bis(ethylbenzothiazole-6-sulfonic acid) diammonium salt (ABTS) method. The dried adhesive was ground into 200 mesh powder using a grinder and then prepared into a 50 μg / mL sample solution using ultrapure water. 7.4 mM ABTS and 2.6 mM potassium persulfate were mixed in equal volumes to obtain an ABTS free radical solution. Then, 2 mL of the ABTS free radical solution and 2 mL of different sample solutions were mixed evenly in a 5 mL container, and the absorbance of the resulting solution at 731 nm was measured. The total antioxidant capacity of the adhesive was calculated according to (A0-A i ) / A0 is calculated and converted into a percentage, where A0 is the absorbance of the solution obtained after ultrapure water treatment, A i is the absorbance of the solution obtained after different sample treatments. The test results are shown in Fig. 9 and Fig.10 .

[0187] from Figure 1It can be seen that the dry bonding strength of the adhesives of Examples 1-5 is significantly improved compared with the adhesive of Comparative Example 1, especially the dry bonding strength of Example 2 is increased to 2.71 MPa. This is because the functionalized seaweed nanofibers serve as a cross-linked skeleton, forming covalent bonds and hydrogen bonds with soy protein through the phenolic hydroxyl and quinone groups of the gallic acid interface platform, increasing the intermolecular cohesion, thereby improving the dry bonding strength of the adhesive.

[0188] from Figure 1 It can be seen that the dry bonding strength of the adhesives of Examples 1-5 is significantly increased compared with the adhesive of Comparative Example 2. This is because compared with ordinary seaweed nanofibers, the gallic acid in the functionalized seaweed nanofibers acts as an interface platform to improve the interfacial interaction between seaweed nanofibers and soy protein, thereby constructing a more stable cross-linked structure.

[0189] from Figure 1 It can be seen that the dry bonding strength of the adhesives in Examples 1-5 is further improved compared with the adhesive in Comparative Example 3. This is because the introduced Fe 3+ Chelated bonds were formed with functionalized seaweed nanofibers and soy protein, increasing the cross-linking density of the adhesive.

[0190] from Figure 1 It can be seen that compared with the adhesive of Comparative Example 4, the dry bonding strength of the adhesives of Examples 1-5 is increased. This is because the gallic acid functionalized platform plays an interfacial cross-linking role and the seaweed nanofibers play a skeleton reinforcement role, making the adhesive have a denser and stronger cured structure.

[0191] from Figure 2 It can be seen that the fracture toughness of the adhesives in Examples 1-5 is significantly improved compared with the adhesives in Comparative Examples 1-4, especially the fracture toughness of Example 2 is increased to 1.42 MJ / m 3 This is because the functionalized seaweed nanofibers in the adhesive inhibit the crack propagation through crack bridging, crack deflection and crack locking during mechanical strain, thereby increasing the toughness of the adhesive. 3+ Metal chelate bonds were constructed in the adhesive as sacrificial bonds to dissipate energy, further improving the toughness of the adhesive.

[0192] from Figure 3 It can be seen that the viscosity of the adhesives in Examples 1-5 is significantly improved compared with the adhesives in Comparative Examples 1-4, especially the viscosity of Example 2 is increased by 4.1 times. This is because the functionalized seaweed nanofibers, Fe 3+ Hydrogen bonds, coordination bonds and other interactions are formed between the adhesive and the soybean protein. Multiple bonds can improve the adhesive's shear resistance and prevent shear thinning, thereby improving the adhesive's initial viscosity.

[0193] from Figure 4 It can be seen that compared with the adhesives of comparative examples 1-4, the wet bonding strength of the adhesives of examples 1-5 is greatly improved, reaching the II plywood standard (≥0.7MPa), especially the wet bonding strength of example 2 is increased to 1.39MPa, which is because the functionalized seaweed nanofibers, Fe 3+ and soybean protein formed a stable fiber-reinforced multi-cross-linked bionic hierarchical structure through covalent bonds, hydrogen bonds and chelate bonds, which acted as a waterproof barrier to inhibit the intrusion of water, thereby improving the water resistance of the adhesive.

[0194] from Figure 5 It can be seen that the mildew-proof validity period of the adhesives of Examples 1-5 is significantly extended compared with the adhesives of Comparative Examples 1-4, especially the mildew-proof validity period of Example 2 is increased to more than 63 days. This is because the gallic acid in the functionalized seaweed nanofibers has effective mildew-proof properties, and the phenolic hydroxyl groups of gallic acid, especially the ortho-hydroxyl groups, can adhere to fungal cells, destroy or deform the bacterial membrane, increase the permeability of the bacterial membrane, and kill fungi, thereby improving the mildew-proof property of the adhesive. At the same time, the dense bionic hierarchical structure of the adhesive of the example helps to hinder the infiltration and proliferation of moisture and fungi, and prolong the mildew-proof validity period.

[0195] from Figure 6 It can be seen that compared with the adhesives of comparative examples 1-4, the antibacterial rates of the adhesive samples of embodiments 1-5 against the two bacteria are significantly improved, especially the antibacterial rates of the sample of embodiment 2 against the two bacteria increased to 97.7% and 98.6%. This is because the introduced gallic acid has an effective antibacterial effect, and at the same time the dense bionic hierarchical structure inhibits the intrusion of moisture and the proliferation of bacteria, thereby improving the antibacterial properties of the adhesive.

[0196] from Figure 7 and Figure 8 It can be seen that compared with the adhesives of comparative examples 1-4, the limiting oxygen index of the adhesives of examples 1-5 is significantly improved and the maximum heat release rate is significantly reduced, which proves that the flame retardancy of the adhesives is enhanced, especially the limiting oxygen index of example 2 is increased to 35.9%, and the maximum heat release rate of example 2 is reduced to 217.2 kW / m 2 This is because inorganic Fe 3+ During the combustion process, the soy protein molecules are induced to dehydrate and carbonize to form a fireproof char layer. The char layer acts as a physical barrier to prevent the infiltration of external oxygen and delay the thermal decomposition of the internal combustible matrix, inhibiting the continuous spread of the flame, thereby improving the flame retardancy of the adhesive. At the same time, the gallic acid-functionalized seaweed nanofibers in the embodiment increase the density and cross-linking degree of the adhesive, and improve the thermal stability of the adhesive.

[0197] from Fig. 9 and Fig.10 It can be seen that compared with the adhesives of comparative examples 1-4, the antioxidant properties of the adhesives of examples 1-5 are significantly enhanced, the absorbance is significantly reduced, and the total antioxidant capacity is improved, especially the total antioxidant capacity of example 2 is improved to 95.6%. This is because gallic acid contains abundant phenolic hydroxyl groups, especially the ortho-hydroxyl groups therein can achieve antioxidant effects through the transfer of hydrogen atoms and single electrons, thereby improving the antioxidant properties of the adhesive. At the same time, the dense cross-linked structure of the examples also helps to block oxygen from damaging the internal structure of the adhesive, further improving the antioxidant properties of the adhesive.

[0198] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A soybean protein adhesive, characterized in that The invention comprises the following raw material components: soybean protein, water, nano-enhancer and modifier; the nano-enhancer is obtained by modifying the surface of seaweed nano-fibers with gallic acid; The modifier is a metal ion compound.

2. The soybean protein adhesive according to claim 1, characterized in that: The invention comprises the following raw material components in parts by weight: 2-7 parts of soy protein, 14-25 parts of water, 0.4-1.2 parts of nano-enhancer, and 0.2-0.8 parts of modifier; preferably, 2.5-5 parts of soy protein, 16-21 parts of water, 0.6-1.0 parts of nano-enhancer, and 0.4-0.6 parts of modifier; preferably, 3 parts of soy protein, 17 parts of water, 0.6-1.0 parts of nano-enhancer, and 0.4-0.6 parts of modifier.

3. The soybean protein adhesive according to claim 1, characterized in that: The soy protein is soy protein isolate, preferably one or a combination of high temperature soluble soy protein isolate, low temperature soluble soy protein isolate, and defatted soy protein isolate; preferably, the protein content of the soy protein is 91-98wt%, preferably 93-95wt%; Preferably, the particle size of the soy protein is 150-350 mesh, preferably 220-260 mesh.

4. The soybean protein adhesive according to claim 1, characterized in that: The nano-enhancer is made of the following raw materials in parts by weight: 285-315 parts of water, 3.6-10.4 parts of seaweed nanofibers, and 1.8-2.4 parts of gallic acid; preferably 290-310 parts of water, 3.8-9.2 parts of seaweed nanofibers, and 1.9-2.2 parts of gallic acid; preferably 300 parts of water, 4-8 parts of seaweed nanofibers, and 2 parts of gallic acid; preferably, the preparation method of the nano-enhancer comprises: mixing the seaweed nanofibers and water in parts by weight; After uniform mixing, a seaweed nanofiber suspension is obtained, the pH is adjusted to 7.0-8.5, gallic acid is added, stirred for 5.6-7.8 hours, washed with water and dried to obtain; preferably, according to parts by weight, the seaweed nanofibers are added to water and mixed evenly to obtain a seaweed nanofiber suspension, the pH is adjusted to 7.5-8 with a pH buffer regulator, gallic acid is added, stirred at a speed of 600-1000r / min at 23-29°C for 6.1-7.3 hours, washed with water and dried to obtain.

5. The soybean protein adhesive according to claim 1, characterized in that: The metal ion compound is Fe 3+ 、Al 3+ and Cr 3+ Any one or more metal ion compounds, preferably containing Fe 3+ compound, preferably FeCl3.

6. The method for preparing the soybean protein adhesive according to any one of claims 1 to 5, characterized in that: The soy protein, water, nano-enhancer and modifier are mixed and stirred to obtain the soy protein adhesive; Preferably, soy protein is added to water and stirred for a first time to obtain soy protein colloid; a nano-enhancer is added to the obtained soy protein colloid and stirred for a second time to obtain an enhanced soy protein colloid; Adding a modifier to the obtained enhanced soybean protein adhesive and performing a third stirring to obtain a soybean protein adhesive; Preferably, the first stirring is stirring at a speed of 900-1900 r / min at 25-35°C for 20-35 min; preferably, the second stirring is stirring at a speed of 600-1400 r / min at 25-33°C for 15-25 min; preferably, the third stirring is stirring at a speed of 500-1200 r / min at 25-30°C for 10-20 min; Preferably, the nano-enhancer is added to the reaction system in 3-7 times, preferably with an interval of 1-4 minutes between each addition, and preferably the amount added each time is 1 / the number of times of the total amount; preferably, the modifier is added to the reaction system in 1-3 times, preferably with an interval of 5-10 minutes between each addition, and preferably the amount added each time is 1 / the number of times of the total amount.

7. A nano-enhancer, characterized in that: The nano-enhancer is obtained by surface functionalization modification of seaweed nanofibers with gallic acid; preferably, the nano-enhancer is made of raw materials including the following parts by weight: 285-315 parts of water, 3.6-10.4 parts of seaweed nanofibers, and 1.8-2.4 parts of gallic acid; preferably, 290-310 parts of water, 3.8-9.2 parts of seaweed nanofibers, and 1.9-2.2 parts of gallic acid; preferably, 300 parts of water, 4-8 parts of seaweed nanofibers, and 2 parts of gallic acid.

8. The method for preparing the nano-enhancer according to claim 7, characterized in that: include: According to weight proportions, seaweed nanofibers are uniformly mixed with water to obtain a seaweed nanofiber suspension, the pH is adjusted to 7.0-8.5, gallic acid is added and stirred for 5.6-7.8 hours, washed with water and dried to obtain; preferably, according to weight proportions, seaweed nanofibers are added to water and mixed uniformly to obtain a seaweed nanofiber suspension, the pH is adjusted to 7.5-8 with a pH buffer regulator, gallic acid is added, stirred at a speed of 600-1000r / min at 23-29°C for 6.1-7.3 hours, washed with water and dried to obtain.

9. The soy protein adhesive according to claim 4, the nano-enhancer according to claim 7, or the preparation method according to claim 8, characterized in that: The preparation method of the seaweed nanofiber is as follows: treating natural seaweed with alkali and then hydrolyzing it with acid; preferably, adding the natural seaweed into a NaOH aqueous solution, stirring, washing and drying, and then adding the natural seaweed into sulfuric acid, stirring, and washing; preferably, adding 10-15g of natural seaweed into 200-240mL of a 5-8wt% NaOH aqueous solution, stirring at 21-27°C for 24-28h, washing and drying to obtain the seaweed treated with alkali, adding 5-7g of the obtained seaweed treated with alkali into 300-370mL of 55-60wt% sulfuric acid, stirring at 21-27°C for 12-17h, washing and drying to obtain the seaweed nanofiber; preferably, adding 10-15g of natural seaweed into 200-240mL 5-8wt% NaOH aqueous solution, stirring at a speed of 500-900r / min for 24-28h at 21-27°C, washing and drying to obtain alkali-treated seaweed, adding 5-7g of the alkali-treated seaweed to 300-370mL 55-60wt% sulfuric acid, stirring at a speed of 800-1200r / min for 12-17h at 21-27°C, washing and drying to obtain g of the seaweed nanofiber; preferably, the seaweed nanofiber has a length of 500-750nm and a width of 30-62nm; preferably, the natural seaweed is any one or a combination of Sargassum, Fucus, Dulse, Porphyra and Gelidium.

10. Use of the soy protein adhesive according to any one of claims 1 to 5 or the soy protein adhesive prepared by the method according to claim 6 in formaldehyde-free artificial panels.

Citation Information

Patent Citations

  • Preparation and application of binder for negative electrode of lithium ion battery based on tannic acid and derivatives thereof

    CN115172752A

  • High-bio-based mildewproof, antibacterial and water-resistant soybean protein adhesive and application thereof

    CN116814216A

  • Hydrophilicity and hydrophobicity adjustable seaweed-based biodegradable packaging material as well as preparation method and application thereof

    CN117164965A

  • Formaldehyde-Free Adhesives and Lignocellulosic Composites Made from the Adhesives

    US20080213597A1

Cited By

  • Modified protein adhesive based on nano-hybrid dynamic cross-linked network as well as preparation method and application of modified protein adhesive

    CN119639422A

  • Modified protein adhesive based on nano-hybrid dynamic crosslinking network, its preparation method and application

    CN119639422B

  • Preparation method of glue-free glued fiberboard based on metal chelation

    CN120572599A