LYSO Ce scintillating material with Mn doped in silicon lattice, preparation method and application
By doped with Mn in the LYSO:Ce scintillation material with Mn doped with Mn, Mn2+ ions suppress the trap energy level and Ce3+/Ce4+ ions occupy the rare earth lattice, forming a C2/c space group, solving the high afterglow level and attenuation in the prior art. The problem of long time has achieved higher light yield and faster attenuation time, suitable for high-energy physical detection and nuclear medical imaging.
Patent Information
- Application Number
- CN202410716182.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-11-12
AI Technical Summary
Existing cerium-doped yttrium silicate (LYSO:Ce) scintillation crystals have problems with high afterglow levels and long attenuation time in medical imaging, which affects signal acquisition efficiency and image quality.
By doping Mn at the silicon lattice, a scintillation material of Lu2(1-x-y)Ce2xY2ySi1-zMnzO5 is formed. The Mn2+ ions suppress the trap energy level of the crystal. Ce3+/Ce4+ ions occupy the rare earth lattice and the space group is C2/c. The growth of single crystals by lafari, bubble generation, mode guide or optical floating zone method significantly reduces the afterglow level and attenuation time.
It significantly reduces the afterglow level, improves the light yield and shortens the attenuation time, improves the comprehensive performance of scintillation materials, and is suitable for high-energy physical detection and nuclear medical imaging and other fields.
Smart Images

Figure CN118931538A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of materials, and in particular to a LYSO Ce scintillation material doped with Mn at a silicon lattice, a preparation method and an application thereof. Background Art
[0002] Time-of-flight-positron emission tomography (TOF-PET) is an important development direction of medical imaging technology, and time resolution is its core indicator. In order to optimize this performance as much as possible, the scintillation crystal needs to have the highest possible light yield and the fastest possible decay time. Among the existing scintillation crystals, cerium-doped lutetium yttrium silicate (LYSO:Ce) crystal is a scintillation crystal material with very excellent performance, with a light yield of about 30,000 ph / MeV and a decay time of about 40ns, and has been widely used in PET.
[0003] Further improvement of the performance of LYSO:Ce scintillation crystals is of great significance to the field of modern nuclear medicine imaging. Specifically, improving its scintillation performance means higher light yield (number of photons / unit energy input), which can more effectively convert gamma photons generated by radioisotope decay into visible light signals, thereby improving signal acquisition efficiency and image quality. This helps doctors obtain clearer and more accurate images of metabolic activities in the body, which is beneficial for early diagnosis of diseases and evaluation of treatment effects.
[0004] In this regard, our company plans to launch a project to further research and develop scintillation crystals to improve their performance, such as increasing light yield, reducing decay time or lowering afterglow levels. Summary of the invention
[0005] To solve at least one of the above technical defects, the present invention provides the following technical solutions:
[0006] The first aspect of the present application document discloses a LYSO:Ce scintillating material doped with Mn in a silicon lattice, wherein the material composition ratio of the scintillating material is: Lu 2(1-x-y) Ce 2x Y 2y Si 1-z Mn z O5, where 0<x≤0.005, 0<y≤0.3, 0<z≤0.003.
[0007] Further, 0.0002≤x≤0.002, 0.05≤y≤0.2.
[0008] Further, 0.0001≤z≤0.0005.
[0009] Furthermore, the space group of the scintillating material is C2 / c.
[0010] The second aspect of the present application document discloses a method for preparing a LYSO:Ce scintillating material doped with Mn at a silicon lattice, characterized in that it comprises the following steps:
[0011] (1) Lu2O3, Y2O3, SiO2, MnO2, and CeO2 are weighed and mixed according to the structural formula shown above to obtain a mixed powder;
[0012] (2) subjecting the obtained mixed powder to a solid phase reaction at 1200-2000° C. for 8-16 hours to obtain Ce and Mn co-doped LYSO scintillating polycrystalline powder;
[0013] (3) forming the obtained mixed powder into a cylinder with a diameter of 4-8 mm, pressing it under a pressure of 120-220 MPa, and subjecting it to a solid phase reaction at 1200-2000° C. for 8-16 hours to obtain a Ce and Mn co-doped LYSO scintillating polycrystalline ceramic rod;
[0014] (4) The obtained polycrystalline ceramic rod is heated to melt, and a Ce and Mn co-doped LYSO scintillating material having the structural formula shown in claim 1 is grown and formed.
[0015] Furthermore, in step (4), single crystal growth is carried out by using a Czochralski method, a kyberyzine method, a guided mode method, a micro-pull-down method or an optical floating zone method.
[0016] The third aspect of this application document discloses the application of the above-mentioned scintillation material or the scintillation material prepared by the above-mentioned preparation method in high-energy physics detection and particle identification or nuclear medicine imaging, such as application in detection devices related to nuclear physics and high-energy physics, application in imaging devices related to nuclear medicine imaging, application in detection devices related to astrophysics, etc.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The present invention designs the scintillating material to partially replace Si lattice sites with Mn. 2+ ions, Mn doping suppresses the trap energy level of the crystal, reducing the crystal afterglow level; Ce occupies the rare earth lattice in the crystal, with Ce 3+ / Ce 4+ It exists in the form of ions with a space group of C2 / c. The scintillating material with this structure has the advantages of short growth cycle, significantly suppressed defects, greatly reduced afterglow level, increased light yield, and reduced decay time. It is suitable for application in high-energy physics detection and particle identification, nuclear medicine imaging and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 The XRD test results of Examples 1-4 are as follows;
[0021] Figure 2 This is the XPS characterization result of Example 4;
[0022] Figure 3 It is the emission spectra of Examples 1-4;
[0023] Figure 4 It is the X-ray excitation emission spectrum of Example 1-4;
[0024] Figure 5 It is the afterglow curve diagram of Examples 1 and 3;
[0025] Figure 6 It is the thermoluminescent spectra of Examples 1 and 3. DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0027] In the preparation of the scintillating material, the purity of the raw materials used is 99.99% (4N) or more, and the silicon-site competitive luminescence doping elements MnO2, CeO2, SiO2, Lu2O3, and Y2O3 are used as raw materials, and the raw material components are mixed in the molar ratio of MnO2:CeO2:SiO2:Lu2O3:Y2O3=z:2x:(1-z):2(1-xy):2y, and fully mixed to obtain a mixed powder. The purity of the raw materials used is 99.99% (4N) or more.
[0028] The powders are mixed evenly and calcined at 1200-2000°C for 8-16 hours to produce a solid phase reaction to obtain polycrystalline powders. The temperature of the solid phase reaction may be 1400-1800°C and the time may be 10-12 hours.
[0029] The obtained mixed powder is pressed into a cylinder with a diameter of 4-8 mm at 120MPa-220MPa, and solid-phase reacted at 1200-2000°C for 8-16 hours. The solid-phase reaction temperature can be 1400-1800°C, the time can be 10-12 hours, and the pressure is preferably 160MPa-200MPa.
[0030] The pressed polycrystalline ceramic rod is used as a material rod and placed in an optical floating zone furnace to melt and recrystallize it through light focusing heating to prepare a single crystal.
[0031] In the single crystal preparation process, the crystal growth method can be a Czochralski method, a kyberyzne method, a guided mold method, a micro-pull-down method, an optical floating zone method, etc., and the atmosphere for single crystal growth can be a mixture of one or more of air, argon, nitrogen, carbon dioxide, and carbon monoxide. Preferably, the crystal growth method is an optical floating zone method, the growth atmosphere is air, and the crystal grows while rotating, with a growth rate of 0.5 to 15 mm / h and a rotation speed of 3 to 20 r / min.
[0032] The following is an exemplary description of the silicon-doped Mn 2+ Preparation method of LYSO:Ce scintillating material with competitive luminescence center. The obtained silicon site doped with Mn 2+ The LYSO:Ce scintillating material of the competing luminescence center is a single crystal.
[0033] Example 1
[0034] A method for preparing a single Ce-doped LYSO standard sample comprises the following steps:
[0035] The single crystal was grown by the optical floating zone method. Lu2O3:CeO2:Y2O3:SiO2 was weighed in a molar ratio of 1.7998:0.0002:0.2:1, mixed thoroughly, and the raw material mixture was subjected to solid phase reaction at 1500°C for 8 hours to obtain scintillating polycrystalline powder.
[0036] The scintillating polycrystalline powder was pressed into a cylindrical rod with a diameter of 6 mm under 180 MPa cold isostatic pressing, and solid phase reaction was carried out at 1400° C. for 10 h to obtain a scintillating polycrystalline ceramic rod.
[0037] The ceramic rod is loaded into the cavity of the optical floating zone furnace, fully melted by light focusing, and then the crystal is grown by moving the melting zone after inoculation to obtain Lu 1.799988 Y 0.2 Ce 0.0002 SiO5 single crystal, wherein the crystal growth adopts the optical floating zone method, the growth atmosphere adopts air, and the crystal grows while rotating, with a growth speed of 10mm / h and a rotation speed of 10r / min.
[0038] Embodiment 2:
[0039] Same as Example 1, except that the molar ratio is Lu2O3:CeO2:Y2O3:SiO2:MnO2=1.7998:0.0002:0.2:0.9999:0.0001.
[0040] Embodiment 3:
[0041] Same as Example 1, except that the molar ratio is Lu2O3:CeO2:Y2O3:SiO2:MnO2=1.7998:0.0002:0.2:0.9995:0.0005.
[0042] Embodiment 4:
[0043] Same as Example 1, except that the molar ratio is Lu2O3:CeO2:Y2O3:SiO2:MnO2=1.7998:0.0002:0.2:0.999:0.001.
[0044] The following table is an analysis of the effects of Examples 1-4:
[0045] Table 1
[0046]
[0047] *Quality factor = light yield / flicker decay time.
[0048] It can be seen from the above table that the present invention increases the light yield of the LYSO:Ce crystal, reduces the scintillation decay time, and effectively improves the comprehensive scintillation performance of the LYSO:Ce crystal, wherein the optimal Mn doping concentration is the doping concentration in Example 3.
[0049] Figure 1 The diffraction peaks of the samples in the examples match well with the standard PDF card (PDF#41-0239) of Lu2SiO5, and no other impurities are introduced. As the Mn co-doping concentration increases, all diffraction peaks move slightly to the direction of small angles, which is related to the replacement of Si by Mn with a larger radius.
[0050] Figure 2 Two obvious signal peaks were detected in the ion source, with the maximum values at 640.98 and 652.31 eV, which are in good agreement with the binding energy values of Mn 2p3 / 2 and Mn 2p1 / 2, respectively. 2+ ion value, it is obvious that Mn 4 + Completely reduced to Mn 2+ .
[0051] Figure 3 The fluorescence spectra of Examples 1-4 (excitation at 358 nm) are shown in Figure 1. The emission peak is Ce. 3+ There is no second emission peak due to the 5d→4f transition of Mn 2+ When the content of the ions is at a preferred value, the fluorescence emission intensity is enhanced.
[0052] Figure 4 The X-ray excitation emission spectra of Examples 1-4 are shown in the figure except Ce3+ The 5d→4f transition emission peak of Mn 2+ From its intensity, it can be seen that Mn 2+ When the content of the ions is at a preferred value, the intensity of X-ray excitation emission is enhanced.
[0053] Figure 5 is the afterglow spectrum of Examples 1 and 3, Mn 2+ When the ion content is at the preferred value, the afterglow level of the crystal will be significantly reduced.
[0054] From the above-mentioned figures, it can be inferred that the luminescence in the scintillation material of the present invention includes scintillation luminescence and photoluminescence. 3+ ions as luminescence centers, and the competitive luminescence center Mn is doped at the silicon site. 2+ Form a competitive relationship with it and realize Ce 3+ Some slow components in the luminous center pass through Ce 3+ →Mn 2+ The radiationless transition energy transfer to Mn 2+ The excited state is then de-excited through a radiation-free process or there is no obvious emission peak in the visible light region, which significantly reduces the slow time component to shorten its time characteristics, thereby reducing the scintillation decay time or afterglow, increasing the light yield, and strengthening the fluorescence emission intensity or X-ray excitation emission intensity.
[0055] Specifically, the luminescence center Ce of the crystal 3+ The ion luminescence is a 5d→4f energy level transition, which is an allowed electric dipole transition, so its decay time is very fast (about 40ns). 4+ After ions are added to Ce:LYSO crystal, they are transferred from oxygen vacancies to Mn 4+ The electron transfer of ions makes Mn 4+ ions are reduced to Mn 2+ . Mn 2+ The Dd electric dipole transition is forbidden by spin and parity, and Mn 2+ The ions are difficult to pump and emit very weakly, with no obvious emission peak in the visible region. 2+ As a competitive luminescence center, new non-radiative transition pathways are introduced, significantly shortening their time characteristics.
[0056] Mn 2+ Replace Si 4+ Then a negatively charged point defect Mn is formed. Si ", so that part of Ce 3+ Converted into stable Ce 4+ To maintain charge balance. 4+The introduction of reduces the efficiency of oxygen vacancies in capturing electrons, inhibits the formation of oxygen vacancies, and thus improves the light output of the crystal.
[0057] Ce 3+ and Mn 2+ There is energy transfer between ions, which reduces the fluorescence lifetime of Ce1 and Ce2 luminescence centers to varying degrees. 2+ Ce doped 4+ Bypassing Ce when emitting light 3+ The process of capturing holes shortens the scintillation process, thereby speeding up the scintillation decay time.
[0058] Mn 2+ The introduction of significantly reduces the TL peak intensity related to oxygen vacancies and afterglow level, reduces the afterglow level of the crystal, and optimizes the scintillation performance of the LYSO:Ce crystal.
[0059] In addition, from the attached Figure 1-5 As shown in Table 1, in the present invention: when Mn 2+ When the ion content is 0.0001≤z≤0.0005, the decay time is shortened, resulting in an increase in light yield, a decrease in afterglow level, and an increase in fluorescence emission intensity or X-ray excitation emission intensity.
[0060] In the present invention, by competing for the luminescence center Mn 2+ Ultrafast luminescence obtained from silicon sites doped with LYSO:Ce scintillating materials can be better applied in high-energy physics detection and particle identification, fast nuclear medical imaging (TOF-PET, PET-CT, PET-MRI) and other fields.
[0061] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A LYSO:Ce scintillating material doped with Mn at the silicon lattice, It is characterized in that Material composition ratio of scintillation material: Lu 2(1-x-y) Ce 2x Y 2y Si 1-z Mn z O 5 , where 0<x≤0.005, 0<y≤0.3, 0<z≤0.
003.
2. A LYSO:Ce scintillating material doped with Mn at the silicon lattice as claimed in claim 1, Features: 0.0002≤x≤0.002, 0.05≤y≤0.
2.
3. The LYSO:Ce scintillating material doped with Mn at the silicon lattice site according to claim 1, Features: 0.0001≤z≤0.0005。 4. The LYSO:Ce scintillating material doped with Mn at the silicon lattice site according to claim 1, Features: The space group of the scintillating material is C2 / c.
5. A method for preparing a LYSO:Ce scintillating material doped with Mn in silicon lattice. It is characterized in that The following steps are involved: (1) Weigh Lu according to the composition ratio shown in claim 1 2 O 3 , Y 2 O 3 、SiO 2 、MnO 2 、CeO 2 and mixing to obtain a mixed powder; (2) subjecting the obtained mixed powder to a solid phase reaction at 1200-2000° C. for 8-16 hours to obtain Ce and Mn co-doped LYSO scintillating polycrystalline powder; (3) forming the obtained mixed powder into a cylinder with a diameter of 4-8 mm, pressing it under a pressure of 120 MPa to 220 MPa, and subjecting it to a solid phase reaction at 1200 to 2000° C. for 8 to 16 hours to obtain a Ce and Mn co-doped LYSO scintillating polycrystalline ceramic rod; (4) The obtained polycrystalline ceramic rod is heated to melt, and a Ce and Mn co-doped LYSO scintillating material having the structural formula shown in claim 1 is grown and formed.
6. The method for preparing a LYSO:Ce scintillating material doped with Mn at a silicon lattice site as claimed in claim 5, It is characterized in that In step (4), single crystal growth is carried out by using the Czochralski method, the kyvo method, the guided mode method, the micro-pull-down method or the optical floating zone method.
7. Use of the scintillating material according to any one of claims 1 to 4 or the scintillating material prepared by the preparation method according to any one of claims 5 to 6 in high energy physics detection and particle identification or nuclear medicine imaging.
Citation Information
Patent Citations
A praseodymium-cerium-doped lutetium pyrosilicate luminescent material and its preparation method
CN102268734A
Rare earth orthosilicate scintillating material with silicon lattice site-doped competitive luminescence center as well as preparation method and application of scintillating material
CN112522787A
Fast attenuation rare earth scintillating material and preparation method thereof
CN118006326A
Rare-Earth Oxyorthosilicates With Improved Growth Stability And Scintillation Characteristics
US20150136992A1
Cited By
Rare earth silicate scintillator material with mixed valence characteristics and preparation and application thereof
CN122917775A