Motor grease composition
By using thickening agents such as reactants of dodecyl stearic acid and organic dibasic acid and amide compounds in motor grease, combined with friction reducing agents, the oxidation and temperature rise of grease in high temperature environments is solved. It significantly extends the service life of the motor and improves its stability.
Patent Information
- Application Number
- CN202310536034.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-12
Smart Images

Figure BDA0004226228780000071 
Figure BDA0004226228780000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lubricating greases, and in particular relates to a motor lubricating grease composition. Background Art
[0002] As an important equipment in modern manufacturing technology, motors are used in various fields of many industries. With the need for continuous operation of equipment by enterprises, the long-term safe and stable operation of motors has become an important factor for an enterprise to create benefits and improve competitiveness. 40% of motor bearing failures are caused by poor lubrication. Improving the quality of grease can increase the life of bearings by 2-5 times. Good lubrication of bearings is one of the important guarantees for safe and stable operation of motors, which in turn helps to extend the life of equipment and minimize the downtime of equipment maintenance.
[0003] In many cases, the effect of heat generation on the life of the grease is greater than the effect of the load on the bearing on the mechanical life. The factor that has the greatest impact on the life of the grease is temperature. Higher bearing temperature rise accelerates the oxidation rate of the grease, and high temperature also increases the volatility of the grease. In addition, as the temperature rises, the grease tends to soften and may become a fluid and leak out of the bearing box.
[0004] Invention patent CN201810538230 discloses a motor bearing grease and a preparation method thereof. The motor bearing grease includes the following components in weight percentage: 35-50 parts of diester oil, 40-48 parts of polyalphaolefin, 10-14 parts of dodecyl stearic acid, and 1-4 parts of additives, wherein the additives include polyethylene glycol and α-phenylnaphthylamine. CN201510065423 discloses a special grease for low-speed motor bearings and a preparation method thereof, which is prepared from the following raw materials in weight parts: 60 parts of dodecyl stearic acid, 40 parts of stearic acid, 38 parts of lithium hydroxide, 3 parts of calcium hydroxide, 10 parts of azelaic acid, 10 parts of sebacic acid, 10 parts of disulfide T322 additive, 5 parts of T406 additive, and 108 parts of base oil. CN201110105616 discloses a submarine motor bearing grease and a preparation method thereof, which uses mixed lithium soap and high-viscosity complex ester thickener. Submarine motor bearing grease has excellent shear stability: it uses double-lipid synthetic base oil with low viscosity to reduce the temperature rise of the bearing after operation; it uses a mixed rust inhibitor to ensure the rust resistance of the bearing when seawater is present. The resulting product has good use effects in corrosion resistance, lubrication stability and load-bearing capacity when used for submarine motor bearings.
[0005] The existing technology mainly focuses on selecting suitable base oils or additives to improve the performance of grease and extend the life of motor bearings. The thickeners used are all ordinary conventional components, and no improvements are made in the thickener components to reduce the temperature rise of motor bearings and increase the lubrication life. Summary of the invention
[0006] The purpose of the present invention is to provide a motor grease composition, which can effectively improve the life of the grease, extend the grease replenishment cycle and the service life of the motor.
[0007] The technical solution adopted by the present invention is that the motor grease composition includes a thickener, a base oil and an additive, specifically: the thickener is 10% to 15%, the base oil is 85% to 90%, and the sum of the mass percentages of the two is 100%; the additive addition ratio is 1% to 5%;
[0008] The thickener consists of mixture A and mixture B:
[0009] a) mixture A is a reactant of 12-hydroxystearic acid, an organic dibasic acid and a saturated aqueous solution of lithium hydroxide monohydrate, wherein the molar ratio of 12-hydroxystearic acid to the organic dibasic acid is 1:0.1-1;
[0010] b) mixture B is an amide compound, wherein the amide compound is a mixture of one or more of dodecylamide, hexadecylamide, octadecylamide, octadecylamide, behenylamide, behenylamide, N,N-dimethyldodecylamide, and N,N'-ethylenebisstearamide in any proportion.
[0011] The present invention is also characterized in that
[0012] The mixture A accounts for 80% to 90% of the total mass of the thickener.
[0013] The organic dibasic acid in the mixture A is a mixture of one or more of C4 to C12 in any proportion.
[0014] The mixture B accounts for 10% to 20% of the total mass of the thickener.
[0015] The base oil is a mixture of one or more of mineral oil, poly-α-olefin, and ester oil in any proportion, and the viscosity grade of the base oil ranges from ISO 46 to ISO320.
[0016] The additive is a mixture of one or more of sulfurized animal and vegetable oils, organic molybdenum compounds, fatty amine derivatives, organic boric acid esters or borate salts.
[0017] When the additive is sulfurized animal and vegetable oil, the added proportion of sulfurized animal and vegetable oil is 0.5% to 2%;
[0018] When the additive is an organic molybdenum compound, the addition ratio of the organic molybdenum compound is 1% to 5%;
[0019] When the additive is a fatty amine derivative, the added proportion of the fatty amine derivative is 0.5% to 2%;
[0020] When the additive is borate, the added proportion of borate is 1% to 3%.
[0021] The beneficial effects of the present invention are:
[0022] The motor grease composition of the present invention can maintain a sufficiently low friction coefficient between the motor bearing friction pairs for a long time, suppress the temperature rise of the motor bearing during operation, and reduce the starting torque at low temperature, thereby effectively improving the life of the grease, extending the grease replenishment cycle and the service life of the motor. The motor grease composition uses metal soap and amide compounds as mixed thickeners, and adds a friction reducer to synergistically enhance the effect, so as to effectively reduce the friction coefficient between the friction pairs and reduce the bearing temperature rise. The motor grease composition of the present invention has outstanding low-temperature starting torque, excellent performance in suppressing bearing temperature rise, and outstanding long-life durability. DETAILED DESCRIPTION
[0023] The present invention is described in detail below in conjunction with specific implementation modes.
[0024] The present invention provides a motor grease composition, comprising a thickener, a base oil and an additive, specifically: the thickener is 10% to 15%, the base oil is 85% to 90%, and the sum of the mass percentages of the two is 100%; the additive addition ratio is 1% to 5% (the additive accounts for 1% to 5% of the sum of the mass of the "thickener" and the "base oil");
[0025] The thickener consists of mixture A and mixture B:
[0026] a) Mixture A is a reactant of dodecyl hydroxystearic acid, an organic dibasic acid and a saturated aqueous solution of lithium hydroxide monohydrate, wherein the molar ratio of 12-hydroxystearic acid to the organic dibasic acid is 1:0.1-1; and mixture A accounts for 80%-90% of the total mass of the thickener.
[0027] The organic dibasic acid in the mixture A is a mixture of one or more of C4 to C12 in any proportion;
[0028] b) mixture B is an amide compound, wherein the amide compound is a mixture of one or more of dodecylamide, hexadecylamide, octadecylamide, octadecylamide, behenylamide, behenylamide, N,N-dimethyldodecylamide, and N,N'-ethylenebisstearamide in any proportion; the mixture B accounts for 10% to 20% of the total mass of the thickener; the base oil is a mixture of one or more of mineral oil, poly-α-olefin, and ester oil in any proportion, and the viscosity grade of the base oil ranges from ISO 46 to ISO320;
[0029] The additive is a mixture of one or more of sulfurized animal and vegetable oils, organic molybdenum compounds, fatty amine derivatives, organic boric acid esters or borates;
[0030] When the additive is sulfurized animal and vegetable oil, the added proportion of sulfurized animal and vegetable oil is 0.5% to 2%;
[0031] When the additive is an organic molybdenum compound, the addition ratio of the organic molybdenum compound is 1% to 5%;
[0032] When the additive is a fatty amine derivative, the added proportion of the fatty amine derivative is 0.5% to 2%;
[0033] When the additive is borate, the added proportion of borate is 1% to 3%.
[0034] Example 1
[0035] 12900g poly-α-olefin (viscosity 100mm 2 / s), 1701g dodecyl hydroxystearic acid, 400g lithium hydroxide monohydrate, 344g sebacic acid and 1500g water are put into the reactor, heated to 80°C and stirred evenly. Then heat to about 135°C and saponify at constant temperature for 45min. Continue to heat to 146°C and release pressure to dehydrate at the same time. After the pressure relief is completed, close the pressure relief valve, quickly heat to 210°C and keep the temperature constant for 10min, slowly cool to 185°C, add 450g amide compound 1 and shear and disperse for 40min, continue to cool to about 80°C, add all additives (alkyl molybdenum thiophosphate) and stir for 1.5 hours, remove from the reactor and grind to obtain the desired product. Sample performance data are shown in Table 1.
[0036] Example 2
[0037] 12900g poly-α-olefin (viscosity 100mm 2 / s), 1701g dodecyl hydroxystearic acid, 400g lithium hydroxide monohydrate, 344g sebacic acid and 1500g water are put into the reactor, heated to 80°C and stirred evenly. Then heat to about 135°C and saponify at constant temperature for 45min. Continue to heat to 146°C and release pressure to dehydrate at the same time. After the pressure relief is completed, close the pressure relief valve, quickly heat to 210°C and keep the temperature constant for 10min, slowly cool to 185°C, add 450g amide compound 2 and shear and disperse for 40min, continue to cool to about 80°C, add all additives (alkyl molybdenum thiophosphate) and stir for 1.5 hours, remove from the reactor and grind to obtain the desired product. Sample performance data are shown in Table 1.
[0038] Example 3
[0039] 12900g poly-α-olefin (viscosity 100mm 2 / s), 1701g dodecyl hydroxystearic acid, 400g lithium hydroxide monohydrate, 344g sebacic acid and 1500g water are put into the reactor, heated to 80°C and stirred evenly. Then heat to about 135°C and saponify at constant temperature for 45min. Continue to heat to 146°C and release pressure to dehydrate at the same time. After the pressure relief is completed, close the pressure relief valve, quickly heat to 210°C and keep the temperature constant for 10min, slowly cool to 185°C, add 150g amide compound 2 and shear and disperse for 40min, continue to cool to about 80°C, add all additives (alkyl molybdenum thiophosphate) and stir for 1.5 hours, remove from the reactor and grind to obtain the desired product. Sample performance data are shown in Table 1.
[0040] Comparative Example 1
[0041] 12900g poly-α-olefin, 1701g dodecyl hydroxystearic acid, 400g lithium hydroxide monohydrate, 344g sebacic acid and 1500g water were put into the reactor, heated to 80℃ and stirred evenly. Then heated to about 135℃ and saponified at constant temperature for 45min. Continue to heat to 146℃ and release pressure to dehydrate at the same time. After the pressure release is completed, close the pressure relief valve, quickly heat to 210℃ and keep the temperature constant for 10min, slowly cool to 185℃, shear disperse for 40min, continue to cool to about 80℃, add all additives and stir for 1.5 hours, remove from the reactor and grind to obtain the desired product. The sample performance data is shown in Table 1.
[0042] Comparative Example 2
[0043] 12900g poly-α-olefin, 1701g dodecyl hydroxystearic acid, 400g lithium hydroxide monohydrate, 344g sebacic acid and 1500g water were put into the reactor, heated to 80°C and stirred evenly. Then heated to about 135°C and saponified at constant temperature for 45min. Continue to heat to 146°C and release pressure to dehydrate. After the pressure release is completed, close the pressure relief valve, quickly heat to 210°C and keep the temperature constant for 10min, slowly cool to 185°C, add 450g amide compound 2 and shear and disperse for 40min, continue to cool to about 80°C, add all additives and stir for 1.5 hours, remove from the reactor and grind to obtain the desired product. The sample performance data is shown in Table 1.
[0044] Comparative Example 3
[0045] 12900g poly-α-olefin, 1701g dodecyl hydroxystearic acid, 400g lithium hydroxide monohydrate, 344g sebacic acid and 1500g water were put into the reactor, heated to 80°C and stirred evenly. Then heated to about 135°C and saponified at constant temperature for 45min. Continue to heat to 146°C and release pressure to dehydrate. After the pressure release is completed, close the pressure relief valve, quickly heat to 210°C and keep the temperature constant for 10min, slowly cool to 185°C, add 450g amide compound 2 and shear and disperse for 40min, continue to cool to about 80°C, add all additives and stir for 1.5 hours, remove from the reactor and grind to obtain the desired product. The sample performance data is shown in Table 1.
[0046] Comparative Example 4
[0047] 12900g poly-α-olefin, 1701g dodecyl hydroxystearic acid, 400g lithium hydroxide monohydrate, 344g sebacic acid and 1500g water were put into the reactor, heated to 80°C and stirred evenly. Then heated to about 135°C and saponified at constant temperature for 45min. Continue to heat to 146°C and release pressure to dehydrate. After the pressure release is completed, close the pressure relief valve, quickly heat to 210°C and keep the temperature constant for 10min, slowly cool to 185°C, add 450g amide compound 2 and shear and disperse for 40min, continue to cool to about 80°C, add all additives and stir for 1.5 hours, remove from the reactor and grind to obtain the desired product. The sample performance data is shown in Table 1.
[0048] Test method:
[0049] The grease composition of the present invention was evaluated for bearing temperature rise suppression, torque reduction and anti-wear performance by the following test methods.
[0050] Bearing temperature rise
[0051] The grease composition is loaded into the actual motor bearing, and the bearing temperature rise test is performed under the following conditions. Under the condition of fixed axial and radial loads, the speed is increased in a step-like manner to examine the temperature rise of the bearing at each speed. The time period of each speed is controlled to be about 1 hour after the temperature stabilizes. The temperature sensor transmits and records the temperature of the two bearings, and the temperature rise data is calculated by subtracting the average value of the room temperature from the temperature of the two bearings at the highest speed.
[0052]
[0053] (2) Anti-wear performance
[0054] The anti-wear performance was evaluated by measuring the wear spot diameter of the steel ball according to the method of SH / T 0204.
[0055] Low temperature torque
[0056] Evaluation is carried out according to the method of SH / T 0338, and low torque performance is evaluated by measuring the operating torque of the bearing at low temperature.
[0057] Table 1 Comparison of grease composition properties
[0058]
[0059] As can be seen from Table 1, the grease composition of the present invention, Examples 1 to 3 in which an amide compound (amide compound 1 is octadecene amide and amide compound 2 is docosene acid amide) and alkyl molybdenum thiophosphates are added, significantly reduce the bearing temperature rise and torque, and have excellent anti-wear properties. Comparative Example 1, in which no amide compound is added, has no obvious effect on suppressing the bearing temperature rise. Comparative Examples 2 to 4, in which other types of friction reducers are added, have insufficient anti-wear properties. The grease composition of the present invention uses metal soap and amide compounds as mixed thickeners, and adds friction reducers for synergistic enhancement, effectively reducing the motor bearing temperature rise, and has a significant anti-wear effect, thereby extending the service life of the motor.
Claims
1. Motor grease composition, It is characterized in that It includes a thickener, a base oil and an additive, specifically: the thickener is 10% to 15%, the base oil is 85% to 90%, and the sum of the mass percentages of the two is 100%; the additive addition ratio is 1% to 5%; The thickener is composed of mixture A and mixture B composition: a) mixture A is a reactant of 12-hydroxystearic acid, an organic dibasic acid and a saturated aqueous solution of lithium hydroxide monohydrate, wherein the molar ratio of 12-hydroxystearic acid to the organic dibasic acid is 1:0.1-1; b) mixture B is an amide compound, wherein the amide compound is a mixture of one or more of dodecylamide, hexadecylamide, octadecylamide, octadecylamide, behenylamide, behenylamide, N,N-dimethyldodecylamide, and N,N'-ethylenebisstearamide in any proportion.
2. The motor grease composition according to claim 1, It is characterized in that The mixture A accounts for 80% to 90% of the total mass of the thickener.
3. The motor grease composition according to claim 1, It is characterized in that The organic dibasic acid in the mixture A is a mixture of one or more of C4 to C12 in any proportion.
4. The motor grease composition according to claim 1, It is characterized in that The mixture B accounts for 10% to 20% of the total mass of the thickener.
5. The motor grease composition according to claim 1, It is characterized in that The base oil is a mixture of one or more of mineral oil, poly-α-olefin, and ester oil in any proportion.
6. The motor grease composition according to claim 1, It is characterized in that The additive is a mixture of one or more of sulfurized animal and vegetable oils, organic molybdenum compounds, fatty amine derivatives, organic boric acid esters or borates.
7. The motor grease composition according to claim 1, It is characterized in that When the additive is sulfurized animal and vegetable oil, the added proportion of sulfurized animal and vegetable oil is 0.5% to 2%; When the additive is an organic molybdenum compound, the addition ratio of the organic molybdenum compound is 1% to 5%; When the additive is a fatty amine derivative, the added proportion of the fatty amine derivative is 0.5% to 2%; When the additive is borate, the added proportion of borate is 1% to 3%.
Citation Information
Patent Citations
Lubricating grease composition
CN101189321A
Lubricating grease special for constant-speed universal joint and preparing method thereof
CN101575548A
Grease composition
CN104145011A
Lubricant grease composition, preparation method therefor and application of lubricant grease composition
CN105733753A
Long-life industrial robot RV reducer lubricating grease and preparation method thereof
CN109810768A