Six-element slag system for large-specification GH738 alloy electroslag smelting and use method of six-element slag system

Through the six-member slag system and specific process parameters for large-scale GH738 alloy electroslag smelting, the tail element deviation and surface quality problems of the electroslag ingot are solved, and the yield rate of the GH738 turbine disc is improved.

CN118932183APending Publication Date: 2024-11-12XIAN JUNENG SUPERALLOY MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411017847.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The production of large GH738 turbine discs is limited by the specifications of electroslag ingots, resulting in severe burn-out of the tail elements of the electroslag ingots, low Zr yield, large deviations of Al and Ti elements, poor surface quality, which affects the yield rate of the cast ingots.

Method used

The pre-slag material of large-scale GH738 alloy electroslag smelting six-membered slag system including CaF2, CaO, Al2O3, MgO, TiO2, ZrO2, SiO2 and FeO is controlled by vacuum induction smelting, annealing treatment and electroslag smelting processes. Smelting parameters such as casting temperature, atmosphere, annealing time and slag spraying method to form stable electroslag ingots.

Benefits of technology

The deviation between the head and tail of the electroslag ingot is significantly reduced, the yield of Zr is improved, the surface quality of the ingot is improved, the surface defects are reduced, and the yield of the ingot is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932183A_ABST
    Figure CN118932183A_ABST
Patent Text Reader

Abstract

The invention discloses a six-membered slag system for large-specification GH738 alloy electroslag smelting and a using method of the six-membered slag system. CaF2-CaO-Al2O3-MgO-TiO2-ZrO2 six-membered slag system pre-melted slag is adopted as slag charge, and the slag charge comprises the following components in percentage by weight: 55%-65% of CaF2, 10%-20% of CaO, 15%-25% of Al2O3, 1%-3% of MgO, 1.0%-2.0% of TiO2, 2%-3% of ZrO2, less than or equal to 0.3% of SiO2 and less than or equal to 0.15% of FeO; a GH738 alloy with the large specification of phi 594 mm is subjected to argon-filled smelting by using a protective atmosphere electroslag furnace, the phenomenon that Al is seriously burnt and Ti is increased at the tail of an electroslag ingot is inhibited by controlling the content of Al2O3, TiO2 and unstable oxides SiO2 and FeO in a slag system, ZrO2 is added into a conventional five-element slag system CaF2-CaO-Al2O3-MgO-TiO2, the problem that Zr is burnt out at the tail of the GH738 electroslag ingot is remarkably relieved, meanwhile, the content of MgO is reduced, and the production cost is reduced. The slag viscosity is reduced, and the surface quality problems such as slag channels and steel seepage points on the surface of the electroslag ingot are solved. After the GH738 alloy with the specification of phi 594 mm smelted by using the slag system is demoulded, the surface quality is obviously improved, the content deviation of Al and Ti elements is reduced to be within 0.05% from 0.15%, and the Zr yield at the tail part of an electroslag ingot is improved to be more than 80% from 50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-temperature alloy smelting, and in particular to a hexavalent slag system for large-scale GH738 alloy electroslag smelting and a use method thereof. Background Art

[0002] With the development of energy and environmental protection, the demand for flue gas turbines in refineries is increasing, and it is developing towards large-scale and high-power. The demand for large-scale flue gas turbines is large. The power of large-scale flue gas turbines is above 30,000 kW, and the required turbine disc diameter is 1250-1500mm. The material is GH738 alloy. GH738 alloy is an age-hardened nickel-based high-temperature alloy. It has good gas corrosion resistance, high yield strength and fatigue resistance, good process plasticity and stable organization.

[0003] At present, the conventional smelting process of high-quality GH738 is a triple smelting process, which uses vacuum induction melting + protective atmosphere electroslag melting + vacuum consumable melting process to obtain (500±20)mm consumable ingots. Therefore, due to the limitation of ingot specifications, only turbine discs with a diameter of less than 1200mm can be produced. Domestic GH738 turbine discs with a diameter greater than 1200mm mainly rely on imports. In recent years, domestic enterprises have begun to develop large-scale GH738 smelting process routes to obtain large-scale large single-weight ingots with consumable ingot diameters of more than 600mm. As the specifications of the finished ingots increase, the electroslag smelting specifications also increase from (450±20)mm to Φ590(±20)mm. The problems brought about by this are: (1) The tail elements of the electroslag ingot are severely burned, and the tail Zr recovery rate is low, only about 50%. The deviation of Al and Ti elements in the head and tail of the electroslag ingot is greater than 0.15%. (2) The surface quality of the electroslag ingot deteriorates, and defects such as pits and steel penetration points appear on the surface of the ingot. The above-mentioned electroslag smelting problems significantly affect the quality of the ingot. The large element deviation leads to an increase in the sawing amount at the tail of the electroslag ingot, and the poor surface quality leads to an increase in the weight removed from the electrode surface. Therefore, the yield of the ingot will be significantly reduced.

[0004] The composition and surface quality of electroslag smelting are mainly related to whether the slag system composition and supporting smelting parameters are appropriate. Therefore, in order to obtain electroslag ingots with uniform and stable composition and good surface quality, it is necessary to develop a large-scale GH738 alloy electroslag smelting six-element slag system and its use method. Summary of the invention

[0005] The object of the present invention is to provide a hexavalent slag system for electroslag smelting of large-scale GH738 alloy and a method of using the same, so as to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for using a six-element slag system for electroslag smelting of a large-scale GH738 alloy, comprising the following steps:

[0007] Step 1: Obtaining GH738 alloy induction ingot by vacuum induction melting (VIM);

[0008] Step 2: annealing the induction cast ingot obtained in step 1;

[0009] Step 3: Surface treatment is performed on the induction ingot obtained after step 1 to form an electroslag electrode;

[0010] Step 4: Use hexavalent slag system pre-melted slag to perform protective atmosphere electroslag smelting to obtain GH738 electroslag ingot.

[0011] Preferably, steps 1 to 4 evolve the VIM and ESR processes into ingots within a specified size range, which is Φ480 (±20) mm-Φ594 (±20) mm.

[0012] Preferably, in the step 1, the GH738 alloy induction ingot has the following chemical composition by mass percentage: C: 0.02%-0.10%, Co: 12%-15%, Mo: 3.5%-5.0%, Cr: 18.0%-21.0%, Ti: 2.75%-3.25%, Al: 1.20%-1.60%, Zr: 0.020%-0.080%, B: 0.003%-0.010%, and the rest is Ni, and the sum of the above mass fraction percentages is 100%.

[0013] Preferably, in step 1, the control requirements for the GH738 alloy induction ingot casting process are:

[0014] (1) The ingot mold is preheated at 450°C for more than 4 hours and assembled before pouring. After assembly, it is placed in the ingot mold chamber, the ingot mold chamber is evacuated to less than 10Pa and pouring is completed within 3 hours;

[0015] (2) Pouring temperature control: 1450-1500℃;

[0016] (3) Pouring atmosphere: The furnace chamber is evacuated to below 10Pa.

[0017] Preferably, the step 2 is to vacuum cool the induction ingot after pouring for 30-120 minutes, and at the same time heat the annealing furnace to 900°C-1200°C for insulation. After the cooling time is reached, the induction ingot mold chamber is emptied, the ingot is taken out and placed in the annealing furnace for a insulation time of 4-16 hours. After the insulation is completed, the ingot is cooled with the furnace to below 600°C and then furnace-cooled.

[0018] Preferably, in step 3, an automatic grinder is used within the circumference of the surface of the induction ingot to process the visible oxide scale and grind it to a surface oxide scale size of ≤15 mm. The end faces of the electrode are cleaned with a handheld grinder until 80% of the area has a metallic luster. At this time, the induction ingot becomes an electroslag electrode.

[0019] Preferably, in step 4, the total weight of the slag added is 100-120 kg, and the slag is added under argon filling conditions using the automatic slag adding device of the equipment, and the argon filling pressure is 0.11-0.15 MPa. 20-40% solid slag is added before smelting, and the remaining slag is evenly added to the crystallizer within 10-30 minutes after arcing for 10-10-30 minutes.

[0020] Preferably, in step 4, a protective atmosphere electric slag furnace is used for smelting, and the argon filling pressure is 0.11-0.15Mpa. The smelting process is divided into three stages: slag and stage, smelting stage and shrinkage feeding stage, wherein:

[0021] The slag stage adopts power + slag resistance control, with a power range of 200-500kW and a slag resistance range of 4.0-6.2mOhm;

[0022] In the smelting stage, melting speed control + slag resistance control is adopted, the electroslag melting speed control range is 250-350kg / h, and the electroslag slag swing control range is 0.1-1.6mOhm;

[0023] The feeding stage adopts power + slag resistance control, with a power range of 350-100kW and a slag resistance range of 4.0-6.2mOhm.

[0024] A six-element slag system for large-size GH738 alloy electroslag smelting comprises: CaF2: 55%-65%, CaO: 10%-20%, Al2O3: 15%-25%, MgO: 1%-3%, TiO2: 1.0%-2.0%, ZrO2: 2%-3%, SiO2≤0.3%, and FeO≤0.15%.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The head and tail composition deviation of the large-sized GH738 alloy electroslag ingot prepared by the present invention is small, which solves the problem of serious burning of Al, Zr and increase of Ti at the tail of the large-sized GH738 electroslag ingot under the conventional electroslag smelting process. The head and tail Al content deviation of the electroslag ingot prepared by the present invention is ≤0.05%, the Ti content deviation is ≤0.05%, and the Zr recovery rate at the tail of the electroslag ingot is ≥80%;

[0027] The large-size GH738 electroslag ingot prepared by the present invention has good surface quality, no surface defects such as steel penetration points, slag grooves, local pits, etc., which solves the problem of large surface treatment loss of ingots caused by poor surface quality and can effectively improve the yield of ingots.

[0028] The present invention provides a method for preparing a large-size GH738 alloy electroslag ingot, comprising the selection of a process route of four steps, namely, vacuum induction melting, induction ingot annealing, electrode surface treatment and electroslag melting, and the setting of process parameters for each step. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The GH738 electroslag ingot smelted by the method of Example 1;

[0030] Figure 2 The GH738 electroslag ingot smelted by the method of Example 2;

[0031] Figure 3 The GH738 electroslag ingot smelted by the method of Example 3;

[0032] Figure 4 GH738 electroslag ingot smelted by comparison method 1;

[0033] Figure 5 These are the operating steps of the method of the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] See also Figure 1-5 The present invention provides a technical solution: a method for using a hexavalent slag system for electroslag smelting of large-scale GH738 alloy, which is specifically implemented according to the following steps:

[0036] Step 1, obtaining a GH738 alloy induction ingot by vacuum induction melting, whose chemical composition, by mass percentage, is: C: 0.02%-0.10%, Co: 12%-15%, Mo: 3.5%-5.0%, Cr: 18.0%-21.0%, Ti: 2.75%-3.25%, Al: 1.20%-1.60%, Zr: 0.020%-0.080%, B: 0.003%-0.010%, and the rest is Ni, and the sum of the above mass fraction percentages is 100%. The control requirements for the induction casting process of GH738 alloy are as follows: (1) The ingot mold is preheated at 450℃ for more than 4 hours, assembled before casting, and after assembly, placed in the ingot mold chamber. The ingot mold chamber is evacuated to less than 10Pa and casting is completed within 3 hours; (2) Pouring temperature control: 1450-1500℃; (3) Pouring atmosphere: The furnace chamber is evacuated to less than 10Pa;

[0037] Step 2, after the pouring, the induction ingot is vacuum cooled for 30-120 minutes, and the annealing furnace is heated to 900°C-1200°C for insulation. After the cooling time is reached, the induction ingot mold chamber is emptied, the ingot is taken out and put into the annealing furnace as soon as possible. The insulation time is 4-16 hours. After the insulation is completed, the ingot is cooled with the furnace to below 600°C and then furnace cooled;

[0038] Step 3: Use an automatic grinder to process the visible oxide scale within the circumference of the surface of the induction ingot until the size of the surface oxide scale is ≤15mm. Use a handheld grinder to clean the end surface of the electrode until 80% of the area has a metallic luster. At this time, the induction ingot becomes an electroslag electrode;

[0039] Step 4, using a protective atmosphere electric slag furnace for smelting, using slag as pre-melted slag, the slag components are CaF2: 55%-65%, CaO: 10%-20%, Al2O3: 15%-25%, MgO: 1%-3%, TiO2: 1.0%-2.0%, ZrO2: 2%-3%, SiO2≤0.3%, FeO≤0.15%.

[0040] The total weight of the slag added is 100-120kg. The slag is added under argon filling conditions using the automatic slag adding device of the equipment. The argon filling pressure is 0.11-0.15Mpa. 20-40% solid slag is added before smelting. After 10-10-30 minutes of arcing, the remaining slag is evenly added to the crystallizer within 10-30 minutes.

[0041] Smelting process parameter control: (1) In the slag melting stage, power + slag resistance control is adopted, the power range is 200-500kW, and the slag resistance range is 4.0-6.2mOhm (2) In the smelting stage, melting rate control + slag resistance control is adopted, the electroslag melting rate control range is 250-350kg / h, and the electroslag slag swing control range is 0.1-1.6mOhm. (3) In the shrinkage feeding stage, power + slag resistance control is adopted, the power range is 350-100kW, and the slag resistance range is 4.0-6.2mOhm

[0042] Example 1

[0043] The present invention provides a method for using a six-element slag system for electroslag smelting of a large-scale GH738 alloy, which is specifically implemented according to the following steps:

[0044] Step 1, obtain GH738 alloy induction ingot by vacuum induction melting, according to the mass percentage, its chemical composition is: C: 0.040%, Co: 12.5%, Mo: 4.5%, Cr: 20.0%, Ti: 3.00%, Al: 1.40%, Zr: 0.060%, B: 0.006%, the rest is Ni, the sum of the above mass fraction percentage is 100%. GH738 alloy induction ingot pouring process control: (1) the ingot mold is preheated at 450℃ for 5h, assembled before pouring, and after assembly, it is put into the ingot mold chamber, the ingot mold chamber is evacuated to 9Pa, and the pouring is completed at 2h30min; (2) pouring temperature control: 1470℃; (3) pouring atmosphere: the furnace chamber is evacuated to 9Pa.

[0045] Step 2, after the pouring is completed, the induction ingot is vacuum cooled for 80 minutes, and the annealing furnace is heated to 1000°C for insulation. After the cooling time is reached, the induction ingot mold chamber is emptied, the ingot is taken out and placed in the annealing furnace as soon as possible. The insulation time is 10 hours. After the insulation is completed, the ingot is cooled with the furnace to below 600°C and then furnace-cooled.

[0046] Step 3: Use an automatic grinder to process the visible oxide scale within the circumference of the surface of the induction ingot until the surface oxide scale size is ≤15mm. Use a handheld grinder to clean the end faces of the electrode until 80% of the area has a metallic luster. At this time, the induction ingot becomes an electroslag electrode.

[0047] Step 4, using a protective atmosphere electric slag furnace for smelting, using slag as pre-melted slag, the slag composition is: CaF2: 59%, CaO: 15%, Al2O3: 20%, MgO: 2%, TiO2: 1.5%, ZrO2: 2.5%, SiO2≤0.3%, FeO≤0.15%. The total weight of the slag added is 120kg, and the slag is added under argon filling conditions using the automatic slag adding device of the equipment, and the argon filling pressure is 0.13Mpa. 30% solid slag is added before smelting, and after 15 minutes of arcing, the remaining slag is evenly added to the crystallizer within 20 minutes.

[0048] Parameter control of smelting process: (1) Power + slag resistance control is adopted in the slag melting stage, and the parameter settings are: time (0-10-20-30-40-50-60min) - power (200-400-500-450-400-350kW) - slag resistance (4.0-5.0-6.2-5.5-5.2-4.6mOhm); (2) Melting rate control + slag resistance control is adopted in the smelting stage, the electroslag melting rate is controlled at 300kg / h, and the electroslag slag swing is controlled at 0.3mOhm. (3) Power + slag resistance control is adopted in the shrinkage compensation stage, time (0-10-20-30-40-50-60min) - power (330-300-200-150-120-100kW) - slag resistance (4.6-5.0-6.2-6.2-7.2-8.6mOhm);

[0049] The composition of the samples was tested at the head and tail of the ingot, and the results are shown in Table 1. Figure 1 .

[0050] Table 1 Composition of GH738 alloy electroslag ingot

[0051]

[0052] Example 2

[0053] The present invention provides a method for using a six-element slag system for electroslag smelting of a large-scale GH738 alloy, which is specifically implemented according to the following steps:

[0054] Step 1, obtain GH738 alloy induction ingot by vacuum induction melting, according to the mass percentage, its chemical composition is: C: 0.040%, Co: 12.5%, Mo: 4.5%, Cr: 20.0%, Ti: 3.00%, Al: 1.40%, Zr: 0.060%, B: 0.006%, the rest is Ni, the sum of the above mass fraction percentage is 100%. GH738 alloy induction ingot pouring process control: (1) the ingot mold is preheated at 450℃ for 5h, assembled before pouring, and after assembly, it is put into the ingot mold chamber, the ingot mold chamber is evacuated to 9Pa, and the pouring is completed at 2h30min; (2) pouring temperature control: 1470℃; (3) pouring atmosphere: the furnace chamber is evacuated to 9Pa.

[0055] Step 2, after the pouring is completed, the induction ingot is vacuum cooled for 80 minutes, and the annealing furnace is heated to 1000°C for insulation. After the cooling time is reached, the induction ingot mold chamber is emptied, the ingot is taken out and placed in the annealing furnace as soon as possible. The insulation time is 10 hours. After the insulation is completed, the ingot is cooled with the furnace to below 600°C and then furnace-cooled.

[0056] Step 3: Use an automatic grinder to process the visible oxide scale within the circumference of the surface of the induction ingot until the surface oxide scale size is ≤15mm. Use a handheld grinder to clean the end faces of the electrode until 80% of the area has a metallic luster. At this time, the induction ingot becomes an electroslag electrode.

[0057] Step 4, using a protective atmosphere electric slag furnace for smelting, using slag as pre-melted slag, the slag composition is: CaF2: 63%, CaO: 15%, Al2O3: 15%, MgO: 2%, TiO2: 2%, ZrO2: 2.5%, SiO2≤0.3%, FeO≤0.15%. The total weight of the slag added is 120kg, and the slag is added under argon filling conditions using the automatic slag adding device of the equipment, and the argon filling pressure is 0.13Mpa. 30% solid slag is added before smelting, and after 15 minutes of arcing, the remaining slag is evenly added to the crystallizer within 20 minutes.

[0058] Parameter control of smelting process: (1) Power + slag resistance control is adopted in the slag melting stage, and the parameter settings are: time (0-10-20-30-40-50-60min) - power (200-400-500-450-400-350kW) - slag resistance (4.0-5.0-6.2-5.5-5.2-4.6mOhm); (2) Melting rate control + slag resistance control is adopted in the smelting stage, the electroslag melting rate is controlled at 300kg / h, and the electroslag slag swing is controlled at 0.3mOhm. (3) Power + slag resistance control is adopted in the shrinkage compensation stage, time (0-10-20-30-40-50-60min) - power (330-300-200-150-120-100kW) - slag resistance (4.6-5.0-6.2-6.2-7.2-8.6mOhm);

[0059] The composition of the samples was tested at the head and tail of the ingot, and the results are shown in Table 2. Figure 2 .

[0060] Table 2 Composition of GH738 alloy electroslag ingot

[0061] element C Co Mo Cr Ti Al Zr B Ni head 0.039 12.51 4.40 20.03 3.03 1.45 0.060 0.0060 Remain tail 0.039 12.50 4.43 20.01 3.04 1.43 0.055 0.0060 Remain

[0062] Example 3

[0063] The present invention provides a method for using a six-element slag system for electroslag smelting of a large-scale GH738 alloy, which is specifically implemented according to the following steps:

[0064] Step 1, obtain GH738 alloy induction ingot by vacuum induction melting, according to the mass percentage, its chemical composition is: C: 0.040%, Co: 12.5%, Mo: 4.5%, Cr: 20.0%, Ti: 3.00%, Al: 1.40%, Zr: 0.060%, B: 0.006%, the rest is Ni, the sum of the above mass fraction percentage is 100%. GH738 alloy induction ingot pouring process control: (1) the ingot mold is preheated at 450℃ for 5h, assembled before pouring, and after assembly, it is put into the ingot mold chamber, the ingot mold chamber is evacuated to 9Pa, and the pouring is completed at 2h30min; (2) pouring temperature control: 1470℃; (3) pouring atmosphere: the furnace chamber is evacuated to 9Pa.

[0065] Step 2, after the pouring is completed, the induction ingot is vacuum cooled for 80 minutes, and the annealing furnace is heated to 1000°C for insulation. After the cooling time is reached, the induction ingot mold chamber is emptied, the ingot is taken out and placed in the annealing furnace as soon as possible. The insulation time is 10 hours. After the insulation is completed, the ingot is cooled with the furnace to below 600°C and then furnace-cooled.

[0066] Step 3: Use an automatic grinder to process the visible oxide scale within the circumference of the surface of the induction ingot until the surface oxide scale size is ≤15mm. Use a handheld grinder to clean the end faces of the electrode until 80% of the area has a metallic luster. At this time, the induction ingot becomes an electroslag electrode.

[0067] Step 4, using a protective atmosphere electric slag furnace for smelting, using slag as pre-melted slag, the slag composition is: CaF2: 59%, CaO: 10%, Al2O3: 25%, MgO: 2%, TiO2: 1%, ZrO2: 2.5%, SiO2≤0.3%, FeO≤0.15%. The total weight of the slag added is 120kg, and the slag is added under argon filling conditions using the automatic slag adding device of the equipment, and the argon filling pressure is 0.13Mpa. 30% solid slag is added before smelting, and after 15 minutes of arcing, the remaining slag is evenly added to the crystallizer within 20 minutes.

[0068] Parameter control of smelting process: (1) Power + slag resistance control is adopted in the slag melting stage, and the parameter settings are: time (0-10-20-30-40-50-60min) - power (200-400-500-450-400-350kW) - slag resistance (4.0-5.0-6.2-5.5-5.2-4.6mOhm); (2) Melting rate control + slag resistance control is adopted in the smelting stage, the electroslag melting rate is controlled at 300kg / h, and the electroslag slag swing is controlled at 0.3mOhm. (3) Power + slag resistance control is adopted in the shrinkage compensation stage, time (0-10-20-30-40-50-60min) - power (330-300-200-150-120-100kW) - slag resistance (4.6-5.0-6.2-6.2-7.2-8.6mOhm);

[0069] The composition of the samples was tested at the head and tail of the ingot, and the results are shown in Table 3. Figure 3 .

[0070] Table 3 Composition of GH738 alloy electroslag ingot

[0071] element C Co Mo Cr Ti Al Zr B Ni head 0.040 12.51 4.40 20.03 3.00 1.40 0.060 0.0060 Remain tail 0.040 12.50 4.41 20.02 3.03 1.37 0.058 0.0060 Remain

[0072] Comparative Example 1

[0073] The present invention provides a method for using a six-element slag system for electroslag smelting of a large-scale GH738 alloy, which is specifically implemented according to the following steps:

[0074] Step 1, obtain GH738 alloy induction ingot by vacuum induction melting, according to the mass percentage, its chemical composition is: C: 0.040%, Co: 12.5%, Mo: 4.5%, Cr: 20.0%, Ti: 3.00%, Al: 1.40%, Zr: 0.060%, B: 0.006%, the rest is Ni, the sum of the above mass fraction percentage is 100%. GH738 alloy induction ingot pouring process control: (1) the ingot mold is preheated at 450℃ for 5h, assembled before pouring, and after assembly, it is put into the ingot mold chamber, the ingot mold chamber is evacuated to 9Pa, and the pouring is completed at 2h30min; (2) pouring temperature control: 1470℃; (3) pouring atmosphere: the furnace chamber is evacuated to 9Pa.

[0075] Step 2, after the pouring is completed, the induction ingot is vacuum cooled for 80 minutes, and the annealing furnace is heated to 1000°C for insulation. After the cooling time is reached, the induction ingot mold chamber is emptied, the ingot is taken out and placed in the annealing furnace as soon as possible. The insulation time is 10 hours. After the insulation is completed, the ingot is cooled with the furnace to below 600°C and then furnace-cooled.

[0076] Step 3: Use an automatic grinder to process the visible oxide scale within the circumference of the surface of the induction ingot until the surface oxide scale size is ≤15mm. Use a handheld grinder to clean the end faces of the electrode until 80% of the area has a metallic luster. At this time, the induction ingot becomes an electroslag electrode.

[0077] Step 4, using a protective atmosphere electric slag furnace for smelting, using slag as pre-melted slag, the slag composition is: CaF2: 59%, CaO: 10%, Al2O3: 20%, MgO: 5%, TiO2: 3.5%, SiO2≤0.60%, FeO≤0.30%. The total weight of the slag added is 120kg, and the slag is added under argon filling conditions using the automatic slag adding device of the equipment, and the argon filling pressure is 0.13Mpa. 30% solid slag is added before smelting, and after 15 minutes of arcing, the remaining slag is evenly added to the crystallizer within 20 minutes.

[0078] Parameter control of smelting process: (1) Power + slag resistance control is adopted in the slag melting stage, and the parameter settings are: time (0-10-20-30-40-50-60min) - power (200-400-500-450-400-350kW) - slag resistance (4.0-5.0-6.2-5.5-5.2-4.6mOhm); (2) Melting rate control + slag resistance control is adopted in the smelting stage, the electroslag melting rate is controlled at 300kg / h, and the electroslag slag swing is controlled at 0.3mOhm. (3) Power + slag resistance control is adopted in the shrinkage compensation stage, time (0-10-20-30-40-50-60min) - power (330-300-200-150-120-100kW) - slag resistance (4.6-5.0-6.2-6.2-7.2-8.6mOhm);

[0079] The composition of the ingot was tested by sampling at the head and tail, and the results are shown in Table 4. It can be seen that the slag composition changes beyond the scope of the present invention, the deviation of Al and Ti content at the head and tail of the electroslag ingot reaches 0.15%, and the Zr element recovery rate is significantly low, only 50%. Figure 4 The surface quality of the electroslag ingot is poor, and there are surface quality defects such as steel penetration points.

[0080] Table 4 GH738 alloy electroslag ingot composition

[0081] element C Co Mo Cr Ti Al Zr B Ni head 0.041 12.52 4.43 20.04 3.00 1.40 0.058 0.0060 Remain tail 0.040 12.50 4.40 20.03 3.16 1.23 0.028 0.0060 Remain

[0082] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for using a six-element slag system for electroslag smelting of large-scale GH738 alloy. Features: The following steps are involved: Step 1: Obtaining GH738 alloy induction ingot by vacuum induction melting (VIM); Step 2: annealing the induction cast ingot obtained in step 1; Step 3: Surface treatment is performed on the induction ingot obtained after step 1 to form an electroslag electrode; Step 4: Use hexavalent slag system pre-melted slag to perform protective atmosphere electroslag smelting to obtain GH738 electroslag ingot.

2. A method for using a hexavalent slag system for electroslag smelting of large-scale GH738 alloy according to claim 1, Features: Steps 1 to 4 evolve the VIM and ESR processes into ingots within a specified size range, which is Φ480 (±20) mm-Φ594 (±20) mm.

3. The method for using the hexavalent slag system for electroslag smelting of large-scale GH738 alloy according to claim 1, Features: In the step 1, the GH738 alloy induction ingot has the following chemical compositions by mass percentage: C: 0.02%-0.10%, Co: 12%-15%, Mo: 3.5%-5.0%, Cr: 18.0%-21.0%, Ti: 2.75%-3.25%, Al: 1.20%-1.60%, Zr: 0.020%-0.080%, B: 0.003%-0.010%, and the rest is Ni, and the sum of the above mass fraction percentages is 100%.

4. The method for using the hexavalent slag system for electroslag smelting of large-scale GH738 alloy according to claim 1, Features: In step 1, the control requirements for the GH738 alloy induction ingot casting process are: (1) The ingot mold is preheated at 450°C for more than 4 hours and assembled before pouring. After assembly, it is placed in the ingot mold chamber, the ingot mold chamber is evacuated to less than 10Pa and pouring is completed within 3 hours; (2) Pouring temperature control: 1450-1500℃; (3) Pouring atmosphere: The furnace chamber is evacuated to below 10Pa.

5. The method for using the hexavalent slag system for electroslag smelting of large-scale GH738 alloy according to claim 1, Features: The step 2 specifically comprises the following steps: vacuum cooling the induction ingot after pouring for 30-120 minutes, and heating the annealing furnace to 900°C-1200°C for insulation. After the cooling time is reached, the induction ingot mold chamber is emptied, and the ingot is taken out and placed in the annealing furnace for a insulation time of 4-16 hours. After the insulation is completed, the ingot is cooled with the furnace to below 600°C and then furnace-cooled.

6. The method for using the hexavalent slag system for electroslag smelting of large-scale GH738 alloy according to claim 1, Features: In step 3, an automatic grinder is used within the circumference of the surface of the induction ingot to process the visible oxide scale until the surface oxide scale size is ≤15mm, and a handheld grinder is used to clean the end faces of the electrode until 80% of the area has a metallic luster. At this time, the induction ingot becomes an electroslag electrode.

7. The method for using the hexavalent slag system for electroslag smelting of large-scale GH738 alloy according to claim 1, Features: In step 4, the total weight of the slag added is 100-120 kg, and the slag is added under argon filling conditions using the automatic slag adding device of the equipment, and the argon filling pressure is 0.11-0.15 MPa. 20-40% solid slag is added before smelting, and the remaining slag is evenly added to the crystallizer within 10-30 minutes after arcing 10-10-30 minutes.

8. The method for using the hexavalent slag system for electroslag smelting of large-scale GH738 alloy according to claim 1, Features: In step 4, a protective atmosphere electric slag furnace is used for smelting, and the argon filling pressure is 0.11-0.15Mpa. The smelting process is divided into three stages: slag and stage, smelting stage and shrinkage feeding stage, wherein: The slag stage adopts power + slag resistance control, with a power range of 200-500kW and a slag resistance range of 4.0-6.2mOhm; In the smelting stage, melting speed control + slag resistance control is adopted, the electroslag melting speed control range is 250-350kg / h, and the electroslag slag swing control range is 0.1-1.6mOhm; The feeding stage adopts power + slag resistance control, with a power range of 350-100kW and a slag resistance range of 4.0-6.2mOhm.

9. The six-element slag system for electroslag smelting of large-scale GH738 alloy according to claim 1, It is characterized in that include: CaF 2 :55%-65%,CaO:10%-20%,Al 2 OR 3 :15%-25%,MgO:1%-3%,TiO 2 :1.0%-2.0%,ZrO 2 :2%-3%,SiO 2 ≤0.3%,FeO≤0.15%。