In-situ nano composite ceramic reinforced aluminum alloy powder for 3D printing and preparation method thereof

By generating Al2O3 and TiB2 phases in situ on the aluminum alloy matrix, combined with induction smelting and atomization powdering technology, the problem of uneven dispersion of nanoceramic particles in aluminum alloy powder is solved, and the fluidity and interface of aluminum alloy powder are improved Combined with strength, the formation of high-performance 3D printed aluminum alloy components is achieved.

CN118932201APending Publication Date: 2024-11-12NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036020.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, nanoceramic particles are difficult to disperse uniformly in aluminum alloy powder, resulting in uneven chemical composition and tissue of 3D printed aluminum alloy components and deterioration of performance. The aluminum alloy powder is prone to deformity after ball milling, and has poor fluidity, which affects 3D printing. Quality of the process.

Method used

B2O3 powder and TiO2 powder react with aluminum alloy matrix to form Al2O3 phase and TiB2 phase. In situ nanocomposite ceramic reinforced aluminum alloy powder is prepared through induction smelting and atomization powder making technology to ensure uniform distribution of ceramic particles and high spherical shape, and improve the The fluidity and interface bonding strength of aluminum alloy powder.

Benefits of technology

The aluminum alloy powder has uniform particle size distribution, high spherical shape, high loose density and excellent fluidity, which significantly improves the comprehensive performance of 3D printed aluminum alloy components and reduces production cycle and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932201A_ABST
    Figure CN118932201A_ABST
Patent Text Reader

Abstract

The invention discloses in-situ nano multiphase ceramic reinforced aluminum alloy powder for 3D printing and a preparation method of the in-situ nano multiphase ceramic reinforced aluminum alloy powder, belongs to the technical field of additive manufacturing, and is used for in-situ preparation of Al2O3 phase and TiB2 ceramic phase reinforced aluminum alloy powder special for 3D printing in combination with an in-situ reaction and atomization powder preparation technology. The nano-particle reinforced aluminum alloy powder prepared through the method has the characteristics of being excellent in comprehensive performance, uniform in particle size distribution, high in sphericity degree, high in apparent density, excellent in fluidity, excellent in metal / ceramic interface bonding and the like, and the requirements of different 3D printing aluminum alloy components can be completely met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of additive manufacturing, and specifically relates to in-situ nano-composite ceramic reinforced aluminum alloy powder for 3D printing and a preparation method thereof. Background Art

[0002] In recent years, with the progress of laser technology and intelligent manufacturing technology, 3D printing technology based on the principle of additive manufacturing has achieved rapid development. 3D printing technology no longer relies on traditional cutting tools, fixtures and molds, but uses spatial three-dimensional models for layer-by-layer manufacturing, with fast forming speed and high precision, thus realizing "free manufacturing". Especially for parts with complex spatial shapes and thin walls, 3D printing technology is more superior, realizing the forming of complex structural parts that are difficult to manufacture by traditional processing methods, and greatly reducing the processing procedures and shortening the processing cycle. Therefore, 3D printing technology has been applied in many fields such as automobiles, aerospace, and medical care, and has been increasingly integrated into social production and life. At present, the metal powders that have been successfully used in 3D printing include aluminum alloys, titanium alloys, steels, and nickel alloys. Among them, aluminum alloys have become a widely used light alloy powder in the field of 3D printing due to their low density, high specific strength, excellent thermal conductivity and corrosion resistance, such as 6061, AlSi10Mg, AlSi12, and Al-Zn.

[0003] As the requirements for comprehensive performance such as strength and wear resistance of 3D printed aluminum alloy parts in the fields of aerospace, automobile manufacturing, etc. continue to increase, single aluminum alloy powder can no longer meet their performance requirements. Due to the excellent reinforcement effect of nano-ceramic particles, many research institutions add nano-ceramic reinforcement particles (such as BC4, TiC, etc.) to aluminum alloy powders through ball milling to obtain 3D printed particle-reinforced aluminum alloy mixed powders to enhance the comprehensive performance of aluminum alloy components. However, due to the huge specific surface area of ​​nano-ceramic particles, their agglomeration effect is obvious and difficult to disperse. The nano-ceramic particles reinforced aluminum alloy mixed powder after ball milling are prone to agglomeration of nano-ceramic particles, which seriously affects the distribution state of nano-particles in the aluminum alloy mixed powder. Even after a long period of ball milling, the agglomeration of nano-ceramic particles cannot be eliminated, which leads to the decrease of chemical composition, uneven organization and comprehensive performance of 3D printed aluminum alloy components. On the other hand, compared with ceramic particles, aluminum alloy powder with lower hardness is easy to deform after ball milling, which is easy to reduce the sphericity of powder, greatly weaken the fluidity and bulk density of aluminum alloy mixed powder in powder bed, increase the difficulty of powder spreading, and cause it to easily produce defects such as pores in the 3D printing process, which has a great impact on the performance of aluminum alloy components. More importantly, the interface wettability between aluminum alloy and nano-ceramic reinforced particles in the ball-milled aluminum alloy mixed powder is poor, and the interface bonding strength is weak. Its 3D printed components are very easy to crack and fail prematurely during service. Therefore, it is particularly important to develop a high-performance, fluidity-excellent nano-ceramic reinforced aluminum alloy powder for 3D printing, which can significantly improve the comprehensive performance of 3D printed aluminum alloy components and has good economic benefits.

[0004] The first method of Chinese patent CN1180383 "TiB2 particle ceramic reinforced aluminum alloy metal matrix composite material" includes the steps of: dispersing a ceramic phase (titanium diboride phase) in aluminum or aluminum alloy liquid, mixing the ceramic phase with cryolite or other fluoride flux powder, and melting the mixture with aluminum or aluminum alloy phase at a temperature between 700°C and 1000°C. In the second method, the fluoride flux is in-situ reduced by molten aluminum or its alloy elements (Mg, Ca) to generate TiB2 microcrystals with different grain sizes and size distributions. The size and size distribution of the microcrystals can be predetermined by determining the flux and alloy composition and process temperature. However, the problem is that the addition of flux Li2TiF6 and LiBF4 causes more slag to appear during the in-situ reaction smelting process, which is difficult to completely remove and is easy to remain in the aluminum alloy to produce impurities, reducing the performance of the aluminum alloy; on the other hand, the flux Li2TiF6 and LiBF4 react in-situ to generate TiB2 ceramic phase, which consumes more energy and more energy. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the present invention provides an in-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing and a preparation method thereof. The nanoparticle-reinforced aluminum alloy powder prepared by the method of the present application has excellent comprehensive performance: uniform particle size distribution, high sphericity, high bulk density, excellent fluidity, excellent metal / ceramic interface bonding, etc., and can fully meet the needs of different 3D printed aluminum alloy components.

[0006] To achieve the above technical objectives, the present invention adopts a specific technical solution, which is an in-situ nano-composite ceramic reinforced aluminum alloy powder for 3D printing, including an aluminum alloy matrix, and Al2O3 phase and TiB2 phase simultaneously grown in-situ on the aluminum alloy matrix.

[0007] As an improved technical solution of the present invention, Al2O3 phase and TiB2 phase are generated on the aluminum alloy matrix by directly reacting B2O3 powder and TiO2 powder with the aluminum alloy matrix, and the molar ratio of B2O3 powder, TiO2 powder and aluminum alloy matrix is ​​1:1:(15~50).

[0008] Another object of the present invention is to provide a method for preparing in-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing, comprising the following steps: Step 1: using induction melting technology, under the protection of inert gas, melting the aluminum alloy block in a crucible at 1200-1900° C. to obtain an aluminum alloy melt; Step 2, weighing B2O3 powder and TiO2 powder according to amount, ball-milling the B2O3 powder and TiO2 powder to mix evenly, and then adding them to the aluminum alloy melt obtained in step 1, and keeping them in a stirring state for 0.5 to 2 hours to promote the in-situ reaction of the B2O3 powder and the TiO2 powder in the aluminum alloy melt, so as to obtain an in-situ complex phase aluminum alloy melt with Al2O3 reinforcement phase and TiB2 reinforcement phase distributed therein; Step 3: by adjusting the temperature of the crucible, the furnace temperature of the in-situ complex phase aluminum alloy melt prepared in step 2 is controlled to be 1500-1650° C., and the in-situ complex phase aluminum alloy melt flowing out of the furnace is processed by atomization powder making technology to obtain spherical in-situ nano-complex phase ceramic reinforced aluminum alloy powder; Step 4: Screen and grade the in-situ nanocomposite ceramic reinforced aluminum alloy powder obtained in step 3 to obtain in-situ nanocomposite ceramic reinforced aluminum alloy powder with a desired particle size.

[0009] As an improved technical solution of the present invention, the inert gas in step one is argon.

[0010] As an improved technical solution of the present invention, the atomization powder making technology in step three adopts an in-situ multiphase aluminum alloy melt that impacts the flow of a supersonic atomization medium; wherein the flow rate of the in-situ multiphase aluminum alloy melt is 0.5 to 2 Kg / min; and the impact pressure of the supersonic atomization medium is 1 to 10 MPa.

[0011] In summary, compared with the prior art, the present invention has the following advantages and beneficial effects: 1. The nanocomposite ceramic reinforced aluminum alloy powder for 3D printing prepared by the present invention, which combines metal smelting and powder preparation technology, has high sphericity and uniform particle size distribution, and has the advantages of excellent fluidity, high bulk density, excellent forming performance, etc., and can fully meet the demand for high-performance aluminum alloy powder required for 3D printing.

[0012] 2. The present invention utilizes aluminum heat in-situ reaction to complete the preparation of uniformly distributed nano-Al2O3 and TiB2 ceramic particle in-situ reinforced aluminum alloy powder (nano-complex ceramic reinforced aluminum alloy powder for 3D printing) in one step. In the process of preparing nano-complex ceramic reinforced aluminum alloy powder for 3D printing, it can control the uniformity of chemical composition, powder particle size uniformity, and the size and content of reinforcing phase particles, etc., which can be used for the forming of 3D printed aluminum alloy components with different performance requirements, and greatly reduce the production cycle and production cost, improve the comprehensive performance of aluminum alloy powder, and have good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a surface morphology of the nano-ceramic particle reinforced aluminum alloy powder particles for 3D printing prepared in Example 1; Figure 2 This is a surface morphology of the nano-ceramic particle reinforced aluminum alloy powder particles for 3D printing prepared in Example 2; Figure 3 This is a surface micro-region morphology of the nano-ceramic particle reinforced aluminum alloy powder particles for 3D printing prepared in Example 2, in which: a-nano Al2O3 ceramic particles, b-nano TiB2 ceramic particles; Figure 4 This is a surface morphology of the aluminum alloy powder particles reinforced with nano-ceramic particles for 3D printing prepared in Example 3; Figure 5 This is a surface morphology of the aluminum alloy powder particles reinforced with nano-ceramic particles for 3D printing prepared in Example 4; Figure 6 This is a surface micro-region morphology of the aluminum alloy powder particles reinforced with nano-ceramic particles for 3D printing prepared in Example 4, in which: c-nano-Al2O3 ceramic particles, d-nano-TiB2 ceramic particles; Figure 7 This is a surface morphology of the aluminum alloy powder particles reinforced with nano-ceramic particles for 3D printing prepared in Example 5; Figure 8 This is a surface micro-region morphology of the aluminum alloy powder particles reinforced with nano-ceramic particles for 3D printing prepared in Example 5, in which: e-nano-Al2O3 ceramic particles, f-nano-TiB2 ceramic particles; Fig. 9 This is a surface morphology of the aluminum alloy powder particles reinforced with nano-ceramic particles for 3D printing prepared in Example 6; Fig.10 This is a surface micro-area morphology of the aluminum alloy powder particles reinforced with nano-ceramic particles for 3D printing prepared in Example 6, in which: g-nano Al2O3 ceramic particles, h-nano TiB2 ceramic particles. DETAILED DESCRIPTION

[0014] In order to make the purpose and technical solution of the embodiment of the present invention clearer, the technical solution of the present invention will be clearly and completely described in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless defined as herein.

[0016] An in-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing includes an aluminum alloy matrix, and Al2O3 phase and TiB2 phase simultaneously grown in-situ on the aluminum alloy matrix. Compared with directly adding dispersed Al2O3 phase and TiB2 phase to the aluminum alloy melt, the Al2O3 phase and TiB2 phase grown in-situ on the aluminum alloy matrix in the present application have good ceramic / aluminum alloy matrix metallurgical interface bonding strength.

[0017] The in-situ nanocomposite ceramic reinforced aluminum alloy powder described in the present application is specifically: B2O3 powder and TiO2 powder are directly reacted with the aluminum alloy matrix to directly and simultaneously generate Al2O3 phase and TiB2 phase on the aluminum alloy matrix. The reaction principle is: 3B2O3+3TiO2+10Al→5Al2O3+3TiB2, wherein the molar ratio of B2O3 powder, TiO2 powder and aluminum alloy matrix is ​​1:1:(15-50).

[0018] It is specifically prepared by the following steps: (1) Raw material configuration: weigh the B2O3, TiO2 oxide powder and aluminum alloy matrix (aluminum alloy block or aluminum alloy powder) in a molar mass ratio of 1:1:15 to 1:1:50 to ensure that the in-situ reaction is fully carried out; (2) Induction melting: place the weighed aluminum alloy block / aluminum alloy powder into a crucible, and then place it in a high-frequency induction furnace (preferably, the preset vacuum degree of the high-frequency induction furnace is better than 0.1 Pa). To prevent oxidation of the aluminum alloy during the melting process, the melting is carried out under the protection of inert argon gas. According to the differences in the physical properties of different types of aluminum alloys, the melting temperature is 1200 to 1900 ° C to ensure that the aluminum alloy is fully melted. After being evenly mixed (ball milling can be used for uniform mixing, stirring and dispersion, and other conventional dispersion techniques can also be used), add it into the aluminum alloy melt, start electromagnetic stirring (to promote the uniform dispersion of B2O3 powder and TiO2 powder in the aluminum alloy powder melt), promote the full in-situ reaction of 3B2O3+3TiO2+10Al→5Al2O3+3TiB2, stir the reaction, and control the time to 0.5-2h (to ensure that it is always in a stirring state during the reaction process, so that the B2O3 and TiO2 powders with a smaller mass fraction can react completely), and then obtain an aluminum alloy melt with Al2O3 (ceramic) phase and TiB2 (ceramic) phase distributed; (3) Atomization powder making: by adjusting the temperature of the heat-insulating crucible, the furnace temperature of the Al2O3 phase and TiB2 phase reinforced aluminum alloy melt is controlled to be 1500-1650°C to obtain a more suitable melt viscosity for easy flow. In order to avoid hollow powder caused by too little melt, the aluminum alloy melt is atomized into fine droplets under the impact of a supersonic atomizing medium (inert argon gas is used here) at a flow rate of 0.5-2 kg / min. In order to ensure the sphericity of the aluminum alloy powder, the atomization pressure (impact pressure generated by the supersonic atomizing medium) is 1-10 MPa. In the process of flying with the atomizing airflow, the droplets are cooled by the atomizing medium (supersonic atomizing medium) to obtain aluminum alloy powder distributed with nano-Al2O3 phase and TiB2 phase (i.e., nano-complex ceramic reinforced aluminum alloy powder); according to Figure 1-9 It is known that the sizes of Al2O3 phase (Al2O3 ceramic reinforcement phase) and TiB2 phase (TiB2 ceramic reinforcement phase) are both nanometer-scale; currently, atomization powder making technology is relatively mature and stable with high efficiency. The present invention combines the thermite reaction with the atomization powder making process to prepare in-situ Al2O3 and TiB2 ceramic phase reinforced aluminum alloy 3D printing special powder.

[0019] (4) Screening and packaging: After cooling the nanocomposite ceramic reinforced aluminum alloy powder, the nanocomposite ceramic reinforced aluminum alloy powder is screened and graded according to the particle size according to different 3D printing performance requirements to obtain nanocomposite ceramic reinforced aluminum alloy powders of different particle sizes (nanocomposite ceramic reinforced aluminum alloy powders of the required particle size can also be obtained), and then packaged and stored.

[0020] Example 1 The in-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing of the present invention is an aluminum alloy powder reinforced by uniformly dispersing in-situ nano Al2O3 and TiB2 ceramic particles (aluminum alloy powder of Al2O3 phase and TiB2 phase grown in-situ on an aluminum alloy matrix), and its preparation method comprises the following steps: (1) Raw material preparation: weigh B2O3, TiO2 powder and aluminum alloy block in a molar mass ratio of 1:1:15; (2) Induction melting: The weighed base aluminum alloy block is placed in a high-frequency induction furnace in a preset vacuum (the preset vacuum degree in this embodiment is 0.05 Pa), and smelting and slag removal are carried out under the protection of inert argon gas. The melting temperature is 1200°C, and B2O3 and TiO2 oxide powders are added to the aluminum alloy melt. Electromagnetic stirring is turned on to promote the in-situ reaction of 3B2O3+3TiO2+10Al→5Al2O3+3TiB2. The reaction time is controlled at 0.5 h to obtain an aluminum alloy melt with nano-Al2O3 and TiB2 ceramic reinforcement phases distributed therein; (3) Atomization powder making: The furnace temperature of the aluminum alloy melt with nano-Al2O3 and TiB2 ceramic reinforcement phase is controlled at 1500-1650°C, and the melt flow rate is set to 0.5 kg / min. The aluminum alloy melt is atomized into fine droplets under the impact of supersonic inert argon atomizing medium. The atomizing pressure is 1 MPa. The droplets are cooled by the atomizing medium while flying with the atomizing airflow to obtain aluminum alloy powder with nano-Al2O3 ceramic reinforcement phase and TiB2 ceramic reinforcement phase (such as the attached Figure 1 As shown); the aluminum alloy powder having nano-Al2O3 ceramic reinforcement phase and TiB2 ceramic reinforcement phase is the nano-complex phase ceramic reinforced aluminum alloy powder; (4) Screening and packaging: After cooling the aluminum alloy powder distributed with nano-Al2O3 ceramic reinforcement phase and TiB2 ceramic reinforcement phase, the aluminum alloy powder particle size is screened and graded according to different 3D printing performance requirements to obtain the required aluminum alloy powder, which is then packaged and stored.

[0021] Example 2 The present embodiment is different from the specific embodiment 1 in that when the mixture is proportioned in step (1), the molar mass ratio of B2O3, TiO2 powder and base aluminum alloy block is controlled to be 1:1:25; in step (3), the melt flow rate is set to 1.5 Kg / min, and the other aspects are the same as those in the specific embodiment 1. The obtained aluminum alloy powder with Al2O3 ceramic reinforcement phase and TiB2 ceramic reinforcement phase (such as the attached Figure 2-3 shown).

[0022] Example 3 The present embodiment is different from the specific embodiment 1 in that the melting temperature is controlled at 1600°C in step (2); the melt flow rate is set at 2 Kg / min in step (3); and the other aspects are the same as those in the specific embodiment 1. The obtained aluminum alloy powder with Al2O3 ceramic reinforcement phase and TiB2 ceramic reinforcement phase (such as the attached Figure 4 shown).

[0023] Example 4 The present embodiment differs from the specific embodiment 3 in that the reaction time is controlled at 1 h in step (2); the melt atomization pressure is set at 5 MPa in step (3); and the other aspects are the same as those in the specific embodiment 3. The obtained aluminum alloy powder with Al2O3 ceramic reinforcement phase and TiB2 ceramic reinforcement phase (such as the attached Figure 5-6 shown).

[0024] Example 5 The present embodiment is different from the specific embodiment 1 in that when the mixture is proportioned in step (1), the molar mass ratio of B2O3, TiO2 oxide powder to the base aluminum alloy block is controlled at 1:1:50; in step (2), the reaction time is set to 2h, and the other aspects are the same as those in the specific embodiment 1. The obtained aluminum alloy powder (such as the attached Figure 7-8 shown).

[0025] Example 6 The present embodiment is different from the specific embodiment 3 in that the melting temperature is controlled at 1900°C in step (2); the atomization pressure is set at 10 MPa in step (3); and the other aspects are the same as those in the specific embodiment 3. The obtained aluminum alloy powder with Al2O3 ceramic reinforcement phase and TiB2 ceramic reinforcement phase (such as the attached Figure 9-10 shown).

[0026] Comparative Example This comparative example prepares in-situ nanocomposite (Al2O3 phase and TiB2 phase) ceramic reinforced Al alloy 3D printing powder based on the principle of thermite reaction and the atomization powder making technology, and tests the powder spreading effect of the powder, aiming to compare the currently widely used ball milling process for preparing nanophase (Al2O3 phase and TiB2 phase) ceramic reinforced Al alloy 3D printing powder, so as to prove the technical advantages of the present invention. After powder spreading under the same conditions, the aluminum alloy powder of the present application has better effect.

[0027] from Figure 3 , 6It can be found from Figures 10 that nano-Al2O3 phase and TiB2 phase ceramic particles generated in situ by thermite reaction between B2O3 and TiO2 oxide powders and aluminum alloy powders are distributed on the surface of the aluminum alloy powders. In addition, the physical properties of the in-situ nano-ceramic particles reinforced aluminum alloy powders prepared by different process parameters are measured, as shown in Table 1, to illustrate that they have high sphericity and fluidity, and can meet the forming requirements of high-performance aluminum alloy powder 3D printing.

[0028] Table 1 Physical properties of in-situ ceramic reinforced aluminum alloy 3D printing powder in the present invention Example Average particle size (μm) Bulk density(g / cm3) Sphericity Example 1 28±1 1.49±0.1 0.90 Example 2 31±1 1.37±0.1 0.81 Example 3 33±1 1.16±0.1 0.78 Example 4 25±1 1.68±0.1 0.92 Example 5 29±1 1.52±0.1 0.86 Example 6 22±1 1.8±0.1 0.95 Under appropriate process parameter conditions, nano-ceramic particles with high sphericity and high bulk density can be obtained to reinforce aluminum alloy powder in situ, ensuring smooth powder delivery and high bulk density during 3D printing, avoiding defects, and obtaining excellent wettability of aluminum alloy / ceramic interface, enhancing its interface bonding strength, which plays an important role in improving the comprehensive performance of 3D printed aluminum alloy components. In the present invention, nano-ceramic particles reinforced aluminum alloy powder are prepared in situ by aluminum thermal reaction to meet the 3D printing forming requirements of high-performance aluminum alloy components; at the same time, the process method is simple and low-cost, which lays the foundation for the localization of high-performance 3D printing special aluminum alloy powder.

[0029] In summary, the existing technology for preparing nano-ceramic particle reinforced aluminum alloy powder is mainly obtained by ball milling, and the powder is simply mixed and directly used for 3D printing. The ball-milled aluminum alloy powder is easy to deform, has low sphericity and poor fluidity, which seriously affects the smoothness of powder laying during 3D printing, and then has an adverse effect on the density, microstructure and performance of 3D printed components. The preparation method of the present invention directly performs induction melting and atomization powder making on the raw materials. The powder has high sphericity, uniform particle size distribution, and excellent powder fluidity, ensuring the formation of a powder layer with high bulk density. In the 3D printing process, the probability of defects is greatly reduced, and the formed components have small shrinkage deformation and high precision, thereby avoiding the adverse effects of powder deformation on the 3D printing process and component performance.

[0030] Existing nano-ceramic particle reinforced aluminum alloy composite powders are based on aluminum alloy powder and ceramic reinforcement phases to achieve a mixing effect through ball milling, but their agglomeration cannot be avoided during the ball milling process, resulting in the chemical composition of the mixed powder, the reinforcement phase and the particle size of the matrix alloy powder being very different, which in turn leads to uneven microstructure of 3D printed components and adverse effects on performance. In the preparation method of the present invention, nano-composite ceramic particle reinforced aluminum alloy powder is generated in one step by in-situ reaction. The ceramic particles are evenly distributed, the chemical composition is consistent, and the powder particle size is uniform. The size and content of the ceramic particles can be controlled by the insulation time and the oxide addition content, respectively, to achieve the controllable size and enhancement ability of the reinforcement phase particles and meet the needs of aluminum alloy powder for 3D printing with different performance requirements. The present invention innovatively uses the in-situ reaction method to generate uniformly distributed nano-ceramic reinforcement phases, which not only reduces the production cycle of the powder and saves production costs, but also improves the comprehensive performance of the aluminum alloy powder and broadens its application field.

[0031] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0032] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. In-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing, characterized in that: It includes an aluminum alloy matrix, and an Al2O3 phase and a TiB2 phase simultaneously grown in situ on the aluminum alloy matrix.

2. The in-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing according to claim 1, characterized in that: Al2O3 phase and TiB2 phase are generated on the aluminum alloy matrix by directly reacting B2O3 powder and TiO2 powder with the aluminum alloy matrix. The molar ratio of B2O3 powder, TiO2 powder and the aluminum alloy matrix is ​​1:1:x, where x is the specific gravity of the aluminum alloy matrix and can be 15 to 50 according to actual conditions.

3. A method for preparing in-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing according to claim 1 or 2, characterized in that: The steps include: Step 1: using induction melting technology, under the protection of inert gas, melting the aluminum alloy block in a crucible at 1200-1900° C. to obtain an aluminum alloy melt; Step 2, weighing B2O3 powder and TiO2 powder according to amount, ball-milling the B2O3 powder and TiO2 powder to mix evenly, and then adding them to the aluminum alloy melt obtained in step 1, and keeping them in a stirring state for 0.5 to 2 hours to promote the in-situ reaction of the B2O3 powder and the TiO2 powder in the aluminum alloy melt, so as to obtain an in-situ complex phase aluminum alloy melt with Al2O3 reinforcement phase and TiB2 reinforcement phase distributed therein; Step 3: by adjusting the temperature of the crucible, the furnace temperature of the in-situ complex phase aluminum alloy melt prepared in step 2 is controlled to be 1500-1650° C., and the in-situ complex phase aluminum alloy melt flowing out of the furnace is processed by atomization powder making technology to obtain spherical in-situ nano-complex phase ceramic reinforced aluminum alloy powder; Step 4: Screen and grade the in-situ nanocomposite ceramic reinforced aluminum alloy powder obtained in step 3 to obtain in-situ nanocomposite ceramic reinforced aluminum alloy powder with a desired particle size.

4. The method for preparing in-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing according to claim 3, characterized in that: In step 1, the inert gas is argon.

5. The method for preparing in-situ nanocomposite ceramic reinforced aluminum alloy powder for 3D printing according to claim 3, characterized in that: The atomization powder making technology in step three uses a supersonic atomization medium to impact the in-situ multiphase aluminum alloy melt; wherein the flow rate of the in-situ multiphase aluminum alloy melt is 0.5-2Kg / min; and the supersonic atomization medium impact pressure is 1-10MPa.