Electric contact material based on PREP plasma rotating electrode atomization and manufacturing method thereof

Silver powder is prepared by PREP plasma rotary electrode atomization technology, combined with thermal isostatic sintering and extrusion molding, and the wetting and density problems of silver tin oxide electrical contact materials are solved, significantly improving the electrical life and anti-welding performance. It meets the electrical performance requirements under high current conditions.

CN118932206APending Publication Date: 2024-11-12ZHEJIANG FUDA ALLOY MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411056499.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing silver and tin oxide electrical contact materials have poor wetting and low density, which leads to difficult processing and short electrical life, and cannot meet the electrical performance requirements under large currents and special load conditions.

Method used

Silver powder is prepared by PREP plasma rotary electrode atomization technology, and mixed with tin oxide powder and additive powder. By thermal isostatic sintering and extrusion forming, a high density and uniform distribution of silver tin oxide material is formed.

Benefits of technology

It improves the density and wettability of the material, extends the electrical life, and achieves excellent anti-welding and burn-out performance under high current conditions, with an electrical life of more than 130,000 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932206A_ABST
    Figure CN118932206A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of electrical material manufacturing, and particularly relates to an electrical contact material based on PREP plasma rotating electrode atomization and a manufacturing method of the electrical contact material. The manufacturing method comprises the following steps that firstly, silver powder is prepared through a PREP plasma rotating electrode atomization technology, then, a plough shovel type powder mixing machine is used for mixing the silver powder and tin oxide powder into silver tin oxide powder, then, the procedures of hot isostatic pressing sintering, hot extrusion, drawing and the like are carried out, a final finished wire is obtained, and the rivet-shaped contact is machined through cold heading. The method has the advantages that the rotating electrode atomization technology is used, the obtained silver powder is good in sphericity degree, high in surface smoothness, good in fluidity and less in agglomeration in the material, the wettability of the silver powder and tin oxide powder is better than that of a product prepared through an existing method, and the prepared electric contact material is excellent in processability and good in stability. And the electric service life is more excellent under the alternating current or direct current condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrical material manufacturing, and in particular relates to an electrical contact material based on PREP plasma rotating electrode atomization and a manufacturing method thereof. Background Art

[0002] Silver-based electrical contact materials have excellent electrical and thermal conductivity. Pure silver contacts have poor wear resistance and low resistance to welding, and cannot meet the electrical performance requirements under high current and special load conditions. In the development process of the electrical contact industry, with the efforts of practitioners and various scientific research institutions, silver-based composite materials with pure silver materials as the matrix and different reinforcement phases added have gradually been developed and widely used. Silver tin oxide is one of them. Under the action of the reinforcement phase with a higher melting point, the silver tin oxide material has excellent resistance to welding, electrical life and arc burn resistance, and is widely used in various relays and contactors. At present, the main methods for preparing AgSnO2 are internal oxidation of alloy, atomization and powder metallurgy. The electrical contact materials produced by the above processes all have poor wettability between silver and oxide particles, agglomeration of oxide particles and low material density, which leads to easy breakage of wire during processing and cracks in the silver layer during the formation of rivet contacts, affecting the yield of the material. When the contacts are in service, bonding and other phenomena will occur, which will cause the relay to fail and have a great impact on the life of the electrical appliance.

[0003] Through the relevant literature search, the patent literature retrieved for preparing silver tin oxide materials is as follows: Patent CN117821791A, a preparation process of a DC transfer resistant silver oxide tin indium oxide electrical contact material, adopts a special alloy particle internal oxidation process, and adds brittle element additives to the formula. The alloy internal oxidation process allows the oxide to be obtained by in-situ reaction with oxygen in the lattice of the silver matrix. In this way, the fine oxide has a good dispersion strengthening effect on the silver matrix. The addition of brittle additives can increase the brittleness of the contact molten liquid bridge, which is beneficial to improving the material's resistance to fusion welding. By adopting special alloy particle internal oxidation and then ingot extrusion, a metallographic structure of "uniform honeycomb perpendicular to the current direction and striped along the current direction" can be obtained. This metallographic structure has a honeycomb-like distribution of oxides perpendicular to the direction of current. There is a difference between the oxides in the honeycomb wall and the inside of the honeycomb, with the oxide content in the honeycomb wall being high and the oxide content in the honeycomb being relatively low. This structure is similar to a "pipeline" for allowing current to pass through, which has less obstruction to current than the uniform distribution of oxides perpendicular to the direction of current. Therefore, under the premise of a certain total oxide content, the honeycomb structure has a small impedance to current. The oxides are distributed in stripes along the direction of current, so that when the arc acts, it can fix the silver matrix and inhibit material transfer and splashing. However, it still cannot solve the problems of uniformity of internal oxide particles of electrical contact materials, wettability of silver and tin oxide particles, material density, and processability.

[0004] In the traditional process of preparing silver tin oxide materials, the wettability of silver and tin oxide particles cannot be solved, and the surface of the finished wire is not treated, resulting in low material density, difficulty in processing, and high contact resistance. As a result, mass production cannot be achieved and the electrical life of the final electrical product is poor. Therefore, there is a need to improve the existing electrical contact material manufacturing process. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and to provide a method for preparing an electrical contact material based on PREP plasma rotating electrode atomization.

[0006] The technical solution adopted by the present invention is as follows: A method for preparing an electrical contact material based on PREP plasma rotating electrode atomization, comprising the following steps: (1) Preparation of silver powder by PREP method: Place the prepared silver rod into the PREP equipment for powder making and start vacuuming. When the vacuum degree reaches 4×10 -3 Pa, start the cooling system, introduce inert gas at the same time, set the plasma gun power to 30-90 kW, the silver rod diameter to 10-15 mm, the silver rod speed to 10000-50000 rad / min, the silver rod feed speed to 0.5-2.0 mm / s, the plasma arc length formed by the plasma gun to 30-90 mm, and the arc column to 20-50 mm; (2) Powder mixing: the silver powder obtained in step 1 is mixed with the prepared tin oxide powder and additive powder in a ratio of 85-92: 7.5-13: 0.5-2, the speed of the powder mixer is set to 20-40 rad / min, and the mixing time is 2-6 h; (3) Hot isostatic pressing sintering: put the mixed powder into a stainless steel sleeve, set the pressure to 150-200MPa, the sintering temperature to 700-800℃, and the holding time to 2-4h; (4) Extrusion: The AgSnO2 ingot obtained in step (3) is heated to 700-800°C using a resistance furnace and formed into a wire with a diameter of 6 mm using an extruder.

[0007] Furthermore, the additive is one or more of In2O3, CuO, Li2O, NiO, and In2O3 rare earth.

[0008] The silver tin oxide electrical contact material is prepared by the method for preparing electrical contact material based on PREP plasma rotating electrode atomization as described above.

[0009] Plasma Rotating Electrode Atomization (PREP) is a technology used to prepare high-purity, high-density spherical powder materials. Its working principle is to use a plasma beam as a heat source to heat the end of a consumable electrode made of metal or alloy to a molten state, and the centrifugal force generated by the high-speed rotation of the electrode throws out the liquid metal and crushes it into fine droplets, which are then condensed into powder. Usually, the following technical effects can be achieved by using plasma rotating electrode atomization powder making: 1. Narrow powder particle size distribution: more controllable particle size, high sphericity; 2. There is basically no hollow powder or satellite powder: the powder quality is high; 3. High cleanliness: reduced impurity content; 4. Small oxygen increment: can be controlled below 50ppm, which improves the purity of the powder.

[0010] The present invention uses PREP technology to prepare silver powder. The prepared silver powder has a narrow particle size distribution, high particle size controllability, less sphericity powder inclusions, high loose density, low surface activity, and good wettability. The silver powder prepared by the process is mixed with tin oxide powder and additive powder. It is unexpectedly found that the silver powder prepared by the PREP technology and the reinforcement phase have good tissue wettability, less internal agglomerates of the material, and higher material density than the existing process materials. There is no problem of fracture during the wire processing process. The rivet-shaped contact finally prepared has high density, so it has a better electrical life under AC or DC conditions. And the prepared electrical contact material has a life of more than 130,000 times under certain current conditions, and has good resistance to welding and burning. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, without paying creative labor, other drawings obtained based on these drawings still belong to the scope of the present invention.

[0012] Figure 1 The gold phase of the materials prepared in Comparative Example (a) and Example 1 (b) is compared. DETAILED DESCRIPTION

[0013] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in further detail below.

[0014] Embodiment 1: A method for manufacturing an electrical contact material based on PREP plasma rotating electrode atomization comprises the following steps: (1) Preparation of silver powder by PREP method: The prepared silver rod is placed in the homemade PREP equipment for powder making and vacuuming is started. When the vacuum degree reaches 4×10 -3 Pa, start the cooling system, introduce inert gas at the same time, set the plasma gun power to 50 kW, the silver rod diameter to 12 mm, the silver rod speed to 20000 rad / min, the silver rod feed speed to 0.9 mm / s, the plasma arc length formed by the plasma gun to 50 mm, and the arc column to 30 mm; (2) Powder mixing: the silver powder obtained in step 1 is mixed with the prepared tin oxide powder and additive powder in a ratio of 85-92: 7.5-13: 0.5-2, the speed of the powder mixer is set to 30 rad / min, and the mixing time is 5 h; (3) Hot isostatic pressing sintering: The mixed powder is placed in a stainless steel sleeve, the pressure is set to 150 MPa, the sintering temperature is 800 °C, and the holding time is 4 h; (4) Extrusion: The AgSnO2 ingot obtained in step (3) is heated to 800°C using a resistance furnace and formed into a wire with a diameter of 6 mm using an extruder; (5) Wire drawing: The wire obtained in step (4) is processed to φ1.2 mm. Embodiment 2: The difference from Example 1 is that the raw material content is different. It is configured according to 10 kg per time, and the input formula ratio is Ag 88wt.%, SnO2 10wt.%, and CuO 2wt%.

[0015] Embodiment 3: The difference from Example 1 and Example 2 is that the input raw material content is different, and it is configured according to 10 kg per time, including 92wt.%, SnO27wt.%, and 1wt% CuO.

[0016] Comparative Example: AgSnO2 alloy powder was prepared by atomization method, and the raw material formula was the same as that in Example 1. Then, hot isostatic pressing, extrusion, and wire drawing steps were performed with the same parameters as in Example 1 to prepare the contact material.

[0017] The above method was used to make AgSnO2 / Cu rivet contacts for simulated electrical performance experiments. The rivet specifications were R4.2x1.5 (0.5) + 2.6x1.7SR15 for the moving contact and F4.2x1.5 (0.5) + 2.6x1.2 for the static contact. The simulated electrical performance experimental conditions were as follows: 250VAC, 10A, closing force 80g, breaking force 50g, contact frequency 30 times / minute; 20VDC, 5A, closing force 80g, breaking force 40g, contact frequency 30 times / minute. The experimental results are shown in Table 1.

[0018] Table 1 Parameter settings and test results of different embodiments and comparative examples Compared with the prepared material, the material prepared by the present invention has no strip oxide agglomeration inside, and the oxide particles are dispersed and evenly distributed, and the overall effect is better than the existing process materials. The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A method for preparing an electrical contact material based on PREP plasma rotating electrode atomization, characterized in that The steps include: (1) Preparation of silver powder by PREP method: Place the prepared silver rod into the PREP plasma rotating electrode atomization equipment for powder making and start vacuuming. When the vacuum degree reaches 4×10 -3 Pa, start the cooling system, introduce inert gas at the same time, set the plasma gun power to 30-90 kW, the silver rod diameter to 10-15 mm, the silver rod speed to 10000-50000 rad / min, the silver rod feed speed to 0.5-2.0 mm / s, the plasma arc length formed by the plasma gun to 30-90 mm, and the arc column to 20-50 mm; (2) Powder mixing: the silver powder obtained in step 1 is mixed with the prepared tin oxide powder additive powder in a ratio of 85-92: 7.5-13: 0.5-2, the speed of the powder mixer is set to 20-40 rad / min, and the mixing time is 2-6 hours; (3) Hot isostatic pressing sintering: put the mixed powder into a stainless steel sleeve, set the pressure to 150-200MPa, the sintering temperature to 700-800℃, and the holding time to 2-4h; (4) Extrusion: The AgSnO2 ingot obtained in step (3) is heated to 700-800°C using a resistance furnace and formed into a wire with a diameter of 6 mm using an extruder.

2. The method for manufacturing an electrical contact material based on PREP plasma rotating electrode atomization according to claim 1, characterized in that: The additive is one or more of indium oxide, bismuth oxide, copper oxide and rare earth.

3. A silver tin oxide electrical contact material prepared by the method for preparing an electrical contact material based on PREP plasma rotating electrode atomization as described in any one of claims 1 to 2.