Metal composite material and preparation method and application thereof

By forming an intermetallic compound protective layer of Al element on the surface of the iron-based electrothermal alloy matrix, the problem of corrosion-free iron-based electrothermal alloy is solved, the corrosion resistance and electric heating performance are improved, and the service life of the equipment is extended.

CN118932268APending Publication Date: 2024-11-12SHENZHEN GEEKVAPE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410903942.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Iron-based electrothermal alloys are easily corroded in electronic atomization devices, especially due to the corrosion of acid aerosol matrix, which leads to reduced equipment performance and shortened service life.

Method used

An intermetallic compound protective layer containing Al element is formed on the surface of the iron-based electrothermal alloy matrix. The atomic content of Al element is 20% to 40%, and it exists in the form of an intermetallic compound to improve corrosion resistance and maintain electrothermal properties.

Benefits of technology

It significantly improves the corrosion resistance of salt spray and aerosol matrix of metal composites, extends the service life of heating elements and electric heating devices, while maintaining stable electric heating performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932268A_ABST
    Figure CN118932268A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of materials, and particularly relates to a metal composite material and a preparation method and application thereof. The metal composite material comprises an iron-based electrothermal alloy matrix and a protective layer arranged on the surface of the iron-based electrothermal alloy matrix. The protective layer comprises an intermetallic compound, and the protective layer comprises an Al element; the atomic percentage content of the Al element in the protective layer is 20%-40%, and at least part of the Al element exists in the form of an intermetallic compound. Al has excellent corrosion resistance and can resist acid corrosion. According to the embodiment of the invention, the protective layer comprising the intermetallic compound is arranged on the surface of the iron-based electrothermal alloy matrix, the atomic percentage content of the Al element in the protective layer is 20%-40%, and at least part of the Al element exists in the form of the intermetallic compound, so that the corrosion resistance of Al can be effectively exerted, and the service life of the iron-based electrothermal alloy is prolonged. The metal composite material has good salt mist resistance and aerosol matrix corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of material technology, and in particular relates to a metal composite material and a preparation method and application thereof. Background Art

[0002] Electronic atomization devices rely on electrothermal alloys to generate heat. The more commonly used electrothermal alloys include FeCrAl alloys. In FeCrAl alloys, iron accounts for the majority, with an atomic percentage of about 60% to 80%, chromium is about 20% to 30%, and aluminum is 4% to 10%. The presence of a large amount of iron will lead to the following problems: the aerosol matrix used to generate aerosols in electronic atomization devices will come into contact with the electrothermal alloy, and the acidic components in these aerosol matrices will corrode the electrothermal alloy. Summary of the invention

[0003] The purpose of the present application is to provide a metal composite material and a preparation method and application thereof, aiming to solve the problem that iron-based electric heating alloys are easily corroded.

[0004] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0005] In a first aspect, the present application provides a metal composite material, comprising an iron-based electrothermal alloy substrate and a protective layer arranged on the surface of the iron-based electrothermal alloy substrate; the protective layer comprises an intermetallic compound, and the protective layer contains Al element; the atomic percentage of Al element in the protective layer is 20% to 40%, and at least part of the Al element exists in the form of an intermetallic compound.

[0006] Al has excellent corrosion resistance and can resist acid corrosion. In the embodiment of the present application, a protective layer including an intermetallic compound is arranged on the surface of the iron-based electric heating alloy substrate, and the atomic percentage of Al element in the protective layer is 20% to 40%, and at least part of the Al element exists in the form of an intermetallic compound. The protective layer can effectively exert the corrosion resistance of Al, so that the metal composite material has good salt spray resistance and aerosol matrix corrosion resistance.

[0007] At the same time, Al is a metal with high electrical conductivity, and the electrothermal alloy needs to rely on resistance to convert electrical energy into thermal energy, and needs to maintain stable heating during work. Therefore, while improving the corrosion resistance of the metal composite material, it is also necessary to maintain its heating performance. Under the appropriate Al content, the metal composite material of the embodiment of the present application can take into account excellent corrosion resistance and electrothermal performance, so that the metal composite material is not easily corroded by the aerosol matrix when used as an atomizer heating material, and also has a suitable resistance to maintain overall heating stability.

[0008] In some embodiments, the atomic percentage of Al element in the protective layer is 30% to 35%.

[0009] In some embodiments, the thickness of the protective layer is 50-200 μm, and optionally 100-150 μm. With a suitable thickness of the protective layer, the metal composite material can have both excellent corrosion resistance and electrical and thermal properties.

[0010] In some embodiments, the intermetallic compound includes an intermetallic compound formed by one or more elements of Fe, Cr, Ni and Al.

[0011] These intermetallic compounds are similar in composition to the iron-based electrothermal alloy matrix. If they are used as a protective layer, the protective layer and the iron-based electrothermal alloy matrix are more likely to have similar physical properties, such as similar thermal expansion coefficients and similar electrothermal properties, so that the metal composite material has a stable structure (during operation, there will be no cracking problems due to different thermal expansion coefficients in different areas) and stable electrothermal properties.

[0012] In some embodiments, the intermetallic compound includes a ternary AlFeCr intermetallic compound; in the protective layer, the atomic percentage of the Fe element is 48% to 70%, and the atomic percentage of the Cr element is 10% to 15%. Under the above Fe and Cr contents, the protective layer can well improve the corrosion resistance of the metal composite material; at the same time, the protective layer has a high Fe element content, and the Fe element is the main provider of resistance, so the metal composite material can have good electrothermal performance.

[0013] In some embodiments, the protective layer is formed by in-situ reaction of the surface layer of the iron-based electric heating alloy substrate with the Al element. In this way, the protective layer and the iron-based electric heating alloy substrate are tightly combined to form a complete whole, and no gap is formed between the protective layer and the iron-based electric heating alloy substrate, and there is no risk of falling off, which can effectively prevent corrosive substances from contacting the iron-based electric heating alloy substrate through the gap and improve the structural stability of the metal composite material.

[0014] In some embodiments, the iron-based electrothermal alloy matrix includes one or more of FeCrAl alloy and FeCrNi alloy. The solution of the embodiment of the present application is applicable to various iron-based electrothermal alloy matrices and can effectively improve the corrosion resistance of these iron-based electrothermal alloy matrices.

[0015] In a second aspect, the present application provides a method for preparing a metal composite material, comprising the following steps:

[0016] Forming an Al layer on the surface of an iron-based electric heating alloy substrate to obtain an intermediate;

[0017] The intermediate is heat treated under a protective atmosphere to form a protective layer including intermetallic compounds on the surface of the iron-based electrothermal alloy substrate, and the atomic percentage content of Al element in the protective layer is controlled to be 20% to 40%.

[0018] By heat treating the intermediate with an Al layer on the surface, Al atoms diffuse into the surface layer of the iron-based electric heating alloy matrix under the action of heat, and can chemically combine with the metal in the iron-based electric heating alloy matrix to form intermetallic compounds. At the same time, the atomic percentage of the Al element in the protective layer is controlled to be 20% to 40%, which can effectively exert the corrosion resistance of Al and make the metal composite material have good salt spray resistance and aerosol matrix corrosion resistance.

[0019] In some embodiments, the method of forming an Al layer on the surface of an iron-based electric heating alloy substrate comprises: immersing the iron-based electric heating alloy substrate in liquid aluminum.

[0020] In some embodiments, the soaking time is 3 to 5 minutes.

[0021] By adjusting the immersion time, the atomic percentage of the Al element in the protective layer can be controlled to be 20% to 40%, and the thickness of the protective layer can be adjusted at the same time.

[0022] In some embodiments, the heat treatment temperature is 950-1100° C. Under high temperature heat treatment, Al atoms diffuse into the surface layer of the iron-based electrothermal alloy matrix and can chemically combine with the metal in the iron-based electrothermal alloy matrix to form an intermetallic compound.

[0023] In a third aspect, the present application provides a heating element, comprising the metal composite material of the first aspect.

[0024] In a fourth aspect, the present application provides an electric heating device, comprising the metal composite material of the first aspect, or comprising the heating element of the third aspect.

[0025] The metal composite material of the embodiment of the present application has excellent corrosion resistance, and thus can improve the corrosion resistance of the heating element or electric heating device containing the electrothermal alloy, and extend the service life of the heating element or electric heating device. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] Figure 1 is a cross-sectional electron microscope image of the metal composite material of Comparative Example 4;

[0028] Figure 2 is a cross-sectional electron microscope image of the metal composite material of Example 2;

[0029] Figure 3 This is an electron microscope image of the protective layer of the metal composite material of Comparative Example 2. DETAILED DESCRIPTION

[0030] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0031] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0032] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can all mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0033] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0034] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0035] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0036] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0037] A first aspect of an embodiment of the present application provides a metal composite material, comprising an iron-based electrothermal alloy substrate and a protective layer arranged on the surface of the iron-based electrothermal alloy substrate; the protective layer comprises an intermetallic compound, and the protective layer contains Al element; the atomic percentage of Al element in the protective layer is 20% to 40%, and at least part of the Al element exists in the form of an intermetallic compound.

[0038] Intermetallic compounds refer to metals and metals or metals and metalloids (such as H, B, N, S, P, C, Si, etc.) that are combined in a certain proportion to form an alloy composition different from the original metal or metalloid lattice. At least part of the Al element exists in the form of an intermetallic compound, which means that in the protective layer, all Al elements may exist in the form of an intermetallic compound; it is also possible that, in addition to existing in the form of an intermetallic compound, part of Al exists in other forms.

[0039] Al has excellent corrosion resistance and can resist acid corrosion. In the embodiment of the present application, a protective layer including an intermetallic compound is arranged on the surface of the iron-based electric heating alloy substrate, and the atomic percentage of Al element in the protective layer is 20% to 40%, and at least part of the Al element exists in the form of an intermetallic compound. The protective layer can effectively exert the corrosion resistance of Al, so that the metal composite material has good salt spray resistance and aerosol matrix corrosion resistance.

[0040] At the same time, Al is a metal with high electrical conductivity, and the electrothermal alloy needs to rely on resistance to convert electrical energy into thermal energy, and needs to maintain stable heating during work. Therefore, while improving the corrosion resistance of the metal composite material, it is also necessary to maintain its heating performance. Under the appropriate Al content, the metal composite material of the embodiment of the present application can take into account excellent corrosion resistance and electrothermal performance, so that the metal composite material is not easily corroded by the aerosol matrix when used as an atomizer heating material, and also has a suitable resistance to maintain overall heating stability.

[0041] Optionally, the atomic percentage of Al in the protective layer is 30% to 35%. For example, the atomic percentage of Al in the protective layer may include any value among 20%, 25%, 30%, 35%, 40%, or any range between the two.

[0042] In some embodiments, the thickness of the protective layer is 50-200 μm, optionally 100-150 μm, for example, any value among 50 μm, 100 μm, 150 μm, 200 μm or any range therebetween.

[0043] With appropriate protective layer thickness, metal composite materials can have both excellent corrosion resistance and electrical and thermal properties.

[0044] In some embodiments, the intermetallic compound includes an intermetallic compound formed by one or more elements of Fe, Cr, Ni and Al. For example, the intermetallic compound may include one or more of a binary intermetallic compound, an AlFeCr ternary intermetallic compound, and an AlFeNi ternary intermetallic compound formed by any one of Fe, Cr, Ni and Al.

[0045] These intermetallic compounds are similar in composition to the iron-based electrothermal alloy matrix. If they are used as a protective layer, the protective layer and the iron-based electrothermal alloy matrix are more likely to have similar physical properties, such as similar thermal expansion coefficients and similar electrothermal properties, so that the metal composite material has a stable structure (during operation, there will be no cracking problems due to different thermal expansion coefficients in different areas) and stable electrothermal properties.

[0046] In some embodiments, the intermetallic compound includes an AlFeCr ternary intermetallic compound; in the protective layer, the atomic percentage of the Fe element is 48% to 70%, optionally 48% to 63%, optionally 50% to 55%, for example, any value among 48%, 50%, 53%, 55%, 60%, 63%, 65%, 70% or a range between any two of them; the atomic percentage of the Cr element is 10% to 15%, optionally 12% to 14%, for example, any value among 10%, 11%, 12%, 13%, 14%, 15% or a range between any two of them.

[0047] Under the above-mentioned Fe and Cr contents, the protective layer can well improve the corrosion resistance of the metal composite material; at the same time, the protective layer has a high Fe element content, and the Fe element is the main provider of resistance, so the metal composite material can have good electrothermal properties.

[0048] In some embodiments, the protective layer further comprises an impurity element with an atomic percentage of 0-2%, optionally 0-0.5%, and the impurity element comprises one or more of C, Si, and Mn. In addition to the main metal component, the metal composite material generally contains some impurities, which will not affect the performance of the metal composite material at a lower content, or will have a small effect.

[0049] In some embodiments, the protective layer is disposed on the surface of the iron-based electrothermal alloy substrate. Specifically, the protective layer is formed by in-situ reaction of the surface layer of the iron-based electrothermal alloy substrate with the Al element. In this way, the protective layer and the iron-based electrothermal alloy substrate are tightly combined to form a complete whole. There is no gap between the protective layer and the iron-based electrothermal alloy substrate, and there is no risk of falling off. It can effectively prevent corrosive substances from contacting the iron-based electrothermal alloy substrate through the gap, and improve the structural stability of the metal composite material.

[0050] In some embodiments, the iron-based electric heating alloy matrix includes one or more of a FeCrAl alloy and a FeCrNi alloy.

[0051] The chemical composition and atomic percentage of the FeCrAl alloy include: Fe 60% to 80%, Cr 20% to 30%, Al 4% to 10%. For example, the FeCrAl alloy may include one or more of FeCr20Al5 and FeCr25Al5. In the case where the iron-based electrothermal alloy matrix includes the FeCrAl alloy, the intermetallic compound in the protective layer includes an AlFeCr ternary intermetallic compound.

[0052] The chemical composition and atomic percentage of the FeCrNi alloy include: Fe 10% to 50%, Cr 20% to 30%, Ni 30% to 60%. For example, the FeCrNi alloy may include one or more of FeCr26Ni60 and FeCr20Ni35. In the case where the iron-based electrothermal alloy matrix includes the FeCrNi alloy, the intermetallic compound in the protective layer includes an AlFeNi ternary intermetallic compound.

[0053] The solution of the embodiment of the present application is applicable to various iron-based electric heating alloy substrates and can effectively improve the corrosion resistance of these iron-based electric heating alloy substrates.

[0054] A second aspect of the present application provides a method for preparing a metal composite material, comprising the following steps:

[0055] Forming an Al layer on the surface of an iron-based electric heating alloy substrate to obtain an intermediate;

[0056] The intermediate is heat treated under a protective atmosphere to form a protective layer including intermetallic compounds on the surface of the iron-based electrothermal alloy substrate, and the atomic percentage content of Al element in the protective layer is controlled to be 20% to 40%.

[0057] In the embodiment of the present application, by heat treating the intermediate having an Al layer on the surface, under the action of heat, Al atoms diffuse into the surface layer of the iron-based electric heating alloy matrix, and can chemically combine with the metal in the iron-based electric heating alloy matrix to form an intermetallic compound. At the same time, the atomic percentage of the Al element in the protective layer is controlled to be 20% to 40%, which can effectively exert the corrosion resistance of Al, so that the metal composite material has good salt spray resistance and aerosol matrix corrosion resistance.

[0058] In some embodiments, the method of forming an Al layer on the surface of an iron-based electric heating alloy substrate comprises: immersing the iron-based electric heating alloy substrate in liquid aluminum.

[0059] Wherein, the soaking time can be set to 3 to 5 minutes, optionally 3.5 to 4.5 minutes, for example, any point value among 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes or any range between two of them. Liquid aluminum can be obtained by heating solid metal aluminum at 700 to 800°C. During the soaking process, the iron-based electrothermal alloy matrix can be completely immersed in the liquid aluminum, thereby forming a uniform Al layer on the surface of the iron-based electrothermal alloy matrix. By adjusting the soaking time, the atomic percentage of the Al element in the protective layer can be controlled to 20% to 40%, and the thickness of the protective layer can be adjusted at the same time.

[0060] Before forming the Al layer on the surface of the iron-based electrothermal alloy substrate, the iron-based electrothermal alloy substrate is cleaned. For example, the iron-based electrothermal alloy substrate can be polished (for example, polished with 1000-3000 mesh sandpaper), and then cleaned and dried with ethanol. The iron-based electrothermal alloy substrate can be a plate material or a processed heating device.

[0061] In some embodiments, the temperature of the heat treatment is 950-1100° C., optionally 1000-1050° C., for example, any point value among 950° C., 1000° C., 1050° C., 1100° C. or any range therebetween. Under high temperature heat treatment, Al atoms diffuse into the surface layer of the iron-based electrothermal alloy matrix and can chemically combine with the metal in the iron-based electrothermal alloy matrix to form an intermetallic compound.

[0062] After the heat treatment step, a cooling treatment and a polishing treatment (for example, polishing with 1000-3000 grit sandpaper) may be performed.

[0063] In some embodiments, the protective atmosphere includes one or more of vacuum, nitrogen, helium, and argon. The heat treatment is performed under the protective atmosphere to prevent oxidation of the Al layer of the intermediate and the metal in the iron-based electrothermal alloy matrix.

[0064] A third aspect of the embodiments of the present application provides a heating element, comprising the metal composite material of the first aspect.

[0065] Heating elements include heating wires, heating plates, heating sheets, heating tubes, etc.

[0066] A fourth aspect of the embodiments of the present application provides an electric heating device, comprising the metal composite material of the first aspect, or comprising the heating element of the third aspect.

[0067] Electric heating devices include electronic atomization devices, electric stoves, household appliances, etc.

[0068] The metal composite material of the embodiment of the present application has excellent corrosion resistance, and thus can improve the corrosion resistance of the heating element or electric heating device containing the electrothermal alloy, and extend the service life of the heating element or electric heating device.

[0069] The following describes the invention in conjunction with specific embodiments.

[0070] A metal composite material, the preparation method of which comprises the following steps:

[0071] 1) The surface of the FeCrAl alloy substrate was polished with 2000 grit sandpaper, then ultrasonically cleaned in ethanol for 30 min and dried at 80 °C.

[0072] 2) Melting aluminum metal in a ceramic crucible to form liquid aluminum at a heating temperature of about 750°C.

[0073] 3) Immerse the FeCrAl alloy substrate into a crucible so that the liquid aluminum immerses the material for a period of time t.

[0074] 4) After taking out the material, heat treat it in vacuum at temperature T for 24 hours, and polish it with 2000 grit sandpaper after natural cooling.

[0075] The immersion time of step 3) and the heat treatment temperature of step 4) are shown in Table 1 below.

[0076] [Table 1]

[0077] Serial number Immersion time (min) Heat treatment temperature(℃) Example 1 3 950 Example 2 4 1000 Example 3 5 1100 Comparative Example 1 5 940 Comparative Example 2 6 1110 Comparative Example 3 2 1110 Comparative Example 4 No treatment No treatment

[0078] In Table 1, the immersion time and heat treatment of Comparative Example 4 are “no treatment”, indicating that the FeCrAl alloy substrate of Comparative Example 4 has not been immersed in liquid aluminum and heat treated.

[0079] The metal composite materials of Examples 1 to 3 and Comparative Examples 1 to 4 were observed through microstructure observation, and it was found that the overall structure of the metal composite material of Comparative Example 4 was uniform and dense. Figure 1The cross-sectional electron micrograph of the comparative example 4 is shown. However, the surface layer of the metal composite materials of Examples 1 to 3 and Comparative Examples 1 to 3 has a layer of structure different from the FeCrAl alloy matrix. For example, the cross-sectional electron micrograph of the metal composite material of Example 2 is shown in Figure 2 As shown, it can be seen that a protective layer different from the FeCrAl alloy matrix structure appears on the surface of the metal composite material. Elemental analysis using an energy dispersive X-ray spectrometer (EDX) shows that the protective layer mainly comprises a ternary metal compound composed of three metal elements: Al, Fe, and Cr. The element composition and thickness of the protective layer of the metal composite materials of Examples 1 to 3 and Comparative Examples 1 to 4 are shown in Table 2 below.

[0080] [Table 2]

[0081]

[0082] In Table 2, the element composition of Comparative Example 4 is the element composition of the surface layer of the FeCrAl alloy substrate.

[0083] According to Table 2, the metal composite materials of Examples 1 to 3 and Comparative Examples 1 to 3 form a protective layer, which has a higher Al content and a lower Fe content than Comparative Example 4.

[0084] The metal composites were subjected to salt spray, aerosol substrate contact and resistivity tests using the following test methods:

[0085] Salt spray test: refer to GB / T2423.17. During the test, place a 2cm×2cm sheet sample with a thickness of 0.1mm in a salt spray test chamber, and then spray the atomized test solution, which is a 5wt% sodium chloride saline solution, with the pH value adjusted to a neutral range (6-7), and the test temperature is 35°C. Record the time when the sample starts to corrode.

[0086] Aerosol substrate contact test: Soak a 2cm×2cm sheet sample with a thickness of 0.1mm in 100mL of aerosol substrate, use a transparent test container and seal it. Observe the discoloration of the sample surface through the container at regular intervals. Record the time when the sample starts to corrode.

[0087] Among them, the aerosol matrix used in the test of this application is a material that can generate aerosols upon heating, a liquid oily substance, and its main components include: glycerin, propylene glycol, plant flavors, and active ingredients; the mass percentage of each component is: glycerin 40%, propylene glycol 40%, plant flavors 9%, and active ingredients 1%.

[0088] Resistivity test: Use a sheet sample of 2cm×2cm in size and 0.1mm in thickness. After soldering the pins on both sides, use a resistance tester to measure the resistance and calculate the resistivity ρ=RS / L, where ρ is the resistivity of the sample, R is the resistance of the sample, S is the cross-sectional area of ​​the sample, and L is the length of the sample.

[0089] The results are shown in Table 3 below.

[0090] [Table 3]

[0091]

[0092] The test results show that the FeCrAl alloy matrix is ​​not treated in Comparative Example 4, and no protective layer is formed on its surface, resulting in poor resistance to salt spray corrosion and aerosol matrix corrosion. In contrast, the metal composite materials of Examples 1 to 3 can resist salt spray corrosion for 50 to 72 hours, which is 12.5 to 18 times that of Comparative Example 4; the metal composite materials of Examples 1 to 3 can resist aerosol matrix corrosion for 20 to 30 days, which is 20 to 30 times that of Comparative Example 4; after long-term contact with salt spray and aerosol matrix, the metal composite materials of Examples 1 to 3 still maintain their original color and are not prone to discoloration. It can be seen that the metal composite materials of Examples 1 to 3 can significantly improve the corrosion resistance of the electric heating alloy by forming a protective layer with an atomic percentage content of Al reaching 20% ​​to 40% on the surface of the FeCrAl alloy matrix, and the protective layer contains AlFeCr ternary intermetallic compound.

[0093] Although Comparative Examples 1 to 3 also use liquid aluminum to immerse the FeCrAl alloy substrate and perform heat treatment, the atomic percentage of Al in the protective layer formed in Comparative Examples 1 and 3 is too low, only 15% and 19%, which is not enough to significantly improve the corrosion resistance of the metal composite material. The Al content in the protective layer of Comparative Example 2 is too high, and the corrosion resistance of the metal composite material cannot be improved well. It is preliminarily speculated that this is because during the preparation process, the FeCrAl alloy substrate is immersed in liquid aluminum for too long, and too much Al is deposited on the surface of the FeCrAl alloy substrate. Excessive Al cannot form intermetallic compounds, so that the chemical composition of the surface layer of the electric heating alloy contains both AlFeCr ternary intermetallic compounds and a relatively high content of Al element (such as Figure 3 As shown in the white area pointed by the arrow, the cross section of the protective layer of Comparative Example 2 contains more Al element), and this chemical composition is not conducive to improving the corrosion resistance. The more specific mechanism of action needs to be explored.

[0094] Therefore, by forming a protective layer with an atomic percentage of Al reaching 20% ​​to 40% on the surface of the electrothermal alloy substrate, and part of the Al element exists in the form of a metametallic compound, the corrosion resistance of the electrothermal alloy can be significantly improved.

[0095] In addition, the electric heating alloy uses resistance to realize the conversion of electric energy into heat energy, so the resistivity is an important parameter for evaluating the electric heating performance of the electric heating alloy. The test results show that the metal composite materials of Examples 1 to 3 have the same resistivity as that of Comparative Example 4, reflecting that by forming a protective layer with an atomic percentage of Al of 20% to 40% on the surface of the metal composite material and part of the Al element in the form of a metal intermetallic compound, the corrosion resistance of the electric heating alloy can be improved while maintaining good electric heating performance without causing deterioration of the electric heating performance.

[0096] Moreover, in the aerosol substrate contact test, it was found that the aerosol substrate was less likely to change color and taste after contacting the metal composite materials of Examples 1 to 3 than Comparative Examples 1 to 4. It can be seen that by forming a protective layer with an atomic percentage of Al of 20% to 40% on the surface of the electrothermal alloy substrate, and part of the Al element exists in the form of a metal intermetallic compound, the oxidation of the aerosol substrate can be alleviated, and the speed of discoloration and taste change of the aerosol substrate can be slowed down.

[0097] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A metal composite material, characterized in that: It comprises an iron-based electrothermal alloy substrate and a protective layer arranged on the surface of the iron-based electrothermal alloy substrate; the protective layer comprises an intermetallic compound, and the protective layer contains an Al element; the atomic percentage of the Al element in the protective layer is 20% to 40%, and at least part of the Al element exists in the form of the intermetallic compound.

2. The metal composite material according to claim 1, characterized in that: The atomic percentage of the Al element in the protective layer is 30% to 35%.

3. The metal composite material according to claim 1 or 2, characterized in that: The thickness of the protective layer is 50-200 μm.

4. The metal composite material according to claim 3, characterized in that: The thickness of the protective layer is 100-150 μm.

5. The metal composite material according to claim 1 or 2, characterized in that: The intermetallic compound includes an intermetallic compound formed by one or more elements of Fe, Cr, Ni and Al.

6. The metal composite material according to claim 5, characterized in that: The intermetallic compound comprises an AlFeCr ternary intermetallic compound; in the protective layer, the atomic percentage of Fe element is 48% to 70%, and the atomic percentage of Cr element is 10% to 15%.

7. The metal composite material according to claim 1 or 2, characterized in that: The protective layer is formed by in-situ reaction of the surface layer of the iron-based electrothermal alloy substrate and the Al element.

8. The metal composite material according to claim 1 or 2, characterized in that: The iron-based electrothermal alloy matrix includes one or more of FeCrAl alloy and FeCrNi alloy.

9. A method for preparing a metal composite material, characterized in that: The steps include: Forming an Al layer on the surface of an iron-based electric heating alloy substrate to obtain an intermediate; The intermediate is heat treated under a protective atmosphere to form a protective layer including intermetallic compounds on the surface of the iron-based electrothermal alloy substrate, and the atomic percentage content of Al element in the protective layer is controlled to be 20% to 40%.

10. The method for preparing the metal composite material according to claim 9, characterized in that: The method for forming the Al layer on the surface of the iron-based electrothermal alloy substrate comprises: immersing the iron-based electrothermal alloy substrate in liquid aluminum.

11. The method for preparing the metal composite material according to claim 10, characterized in that: The soaking time is 3 to 5 minutes.

12. The method for preparing the metal composite material according to any one of claims 9 to 11, characterized in that: The temperature of the heat treatment is 950-1100°C.

13. A heating element, characterized in that: The metal composite material comprises the metal composite material according to any one of claims 1 to 8.

14. An electric heating device, characterized in that: The invention comprises the metal composite material according to any one of claims 1 to 8, or comprises the heating element according to claim 13.