High-toughness and high-corrosion-resistance AlCoCrFeNiMoV high-entropy alloy with precipitated phase strengthening effect and preparation method of high-toughness and high-corrosion-resistance AlCoCrFeNiMoV high-entropy alloy

By introducing Mo and V elements into AlCoCrFeNi2.1 high-entropy alloy and using cold deformation and heat treatment processes, AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect was prepared, which solved its insufficient thermal sensitivity and corrosion resistance at high temperatures. The problem of this problem has achieved high strength, high plasticity and excellent corrosion resistance, and is suitable for the inner wall materials of waste incineration boilers.

CN118979185APending Publication Date: 2024-11-19GUANGDONG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411097368.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

AlCoCrFeNi2.1 high-entropy alloy has insufficient thermal sensitivity and corrosion resistance at high temperatures, which is difficult to meet the application needs of waste incineration boilers.

Method used

Mo elements were introduced into AlCoCrFeNi2.1 high-entropy alloy to improve high temperature stability and acid corrosion resistance. By introducing V elements, the grains were refined, combined with cold deformation and heat treatment processes, AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect was prepared .

Benefits of technology

It significantly improves the comprehensive mechanical properties of the alloy, has high strength, high plasticity and excellent corrosion resistance, yield strength is not less than 1100MPa, tensile strength is not less than 1300MPa, and its self-corrosion performance in 3.5% NaCl solution is better than that of traditional materials. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979185A_ABST
    Figure CN118979185A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high-entropy alloy materials, and particularly relates to a high-toughness and high-corrosion-resistance AlCoCrFeNiMoV high-entropy alloy with a precipitated phase strengthening effect and a preparation method of the high-toughness and high-corrosion-resistance AlCoCrFeNiMoV high-entropy alloy. The high-entropy alloy is prepared from the following components in percentage by mass: 4.0 to 6.0 percent of Al, 18.0 to 20.0 percent of Co, 15 to 17 percent of Cr, 17.0 to 19.0 percent of Fe, 37.0 to 39.0 percent of Ni, 2.0 to 3.0 percent of Mo and 0.5 to 0.7 percent of V, the biphase FCC + B2 lamellar composite material with excellent performance is prepared by reasonably regulating and controlling alloy components and combining solid solution heat treatment, cold rolling and recrystallization heat treatment of cast ingots. Through the strengthening effect of a precipitated phase, the alloy has excellent yield strength and tensile strength under the condition that high plasticity is kept, meanwhile, the alloy has high acid corrosion resistance, and the alloy is suitable for the inner wall material of the waste incineration boiler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high entropy alloy materials, and specifically relates to a high-strength, toughness and corrosion-resistant AlCoCrFeNiMoV high entropy alloy with precipitation phase strengthening effect and a preparation method thereof. Background Art

[0002] As a multi-principal alloy material, high entropy alloy has many unique characteristics and advantages in terms of microstructure and performance. High entropy alloy has a "high entropy effect" in thermodynamics, which can promote the formation of high entropy solid solution; it has a "hysteresis diffusion effect" in kinetics, and the diffusion coefficient is significantly lower than that of traditional alloys; it has a "lattice distortion effect" in microstructure, which can cause solid solution strengthening and improve strength; it has a "cocktail effect" in performance, which is conducive to optimizing the various properties of the alloy. Therefore, high entropy alloys have broad application prospects. Among them, FCC-type high entropy alloys have good plasticity, but low tensile strength, while BCC-type has high tensile strength, but unsatisfactory plasticity; FCC+BCC dual-phase high entropy alloys can take into account the advantages of soft and hard phase high entropy alloys, and can obtain the comprehensive mechanical properties of two types of high entropy alloys, but the performance is still not enough to meet the requirements of high strength and plasticity. Therefore, if based on the hysteresis diffusion effect and lattice distortion effect of FCC phase high entropy alloys at high temperature, the nanoscale precipitation phase is obtained by cold deformation and heat treatment to make the alloy obtain dispersion strengthening, it is expected to further improve the strength of the alloy.

[0003] For example, AlCoCrFeNi designed by Professor Lu Yiping of Dalian University of Technology 2.1 High-entropy alloys (Lu Y, Dong Y, Guo S, et al. A Promising New Class of High-Temperature Alloys: Eutectic High-Entropy Alloys [J]. Rep, 2014, 4: 6200. DOI: 10.1038 / srep06200.) show uniform and fine lamellar morphology in the cast state, with a tensile strength of more than 1 GPa and a plasticity of up to 17%. This high-entropy alloy that can obtain high strength and high plasticity in the cast state has become one of the most valuable high-entropy alloys for industrial applications. However, despite the AlCoCrFeNi 2.1High entropy alloys have good strength and plasticity in the cast state, but from the perspective of engineering application, they still need to be further improved, because the cast alloys will produce some segregation and shrinkage during the solidification process, making the castings more likely to break or deform when subjected to external forces, affecting the service life and safety performance. The different sizes and shapes of micro-grains also seriously affect the mechanical properties of castings. There are also studies (Chen JL, Feng Z, Xue B, et al. High Ductility Crconi Medium Entropy Alloy Prepared by Liquid Nitrogen Temperature Rolling and Short Time Annealing at Moderate Temperature [J]. SSRN Electronic Journal, 2023. DOI: 10.2139 / ssrn.4231164.) showing that the medium entropy alloy obtained by combining warm rolling and annealing at liquid nitrogen temperature can obtain high strength and plasticity, but due to the disadvantages of liquid nitrogen cold rolling process, it is not suitable for large-scale industrial production and will generate unstable nanocrystalline structure, which seriously restricts the industrial application of high entropy alloys prepared by this process.

[0004] In fact, in order to meet the needs of different usage scenarios, the alloy composition design and preparation process can be improved. From the perspective of organizational control, better mechanical properties can be obtained through solid solution strengthening, nano-precipitation phase strengthening and other means, thereby greatly improving the strength and plasticity of the alloy.

[0005] At present, high entropy alloys are widely used in waste incineration boilers, mainly as the inner wall material of waste incineration boilers. However, due to the complex working environment of waste incineration boilers, it involves many harsh factors such as 850℃ high-temperature combustion, particle wear and acidic gas corrosion. Among them, SO2 and HCl gases produced by waste incineration are the main causes of acid corrosion. Therefore, the inner wall material of the boiler has higher requirements for high entropy alloys, requiring them to have high temperature stability, high strength, high toughness and high corrosion resistance at the same time.

[0006] In summary, if AlCoCrFeNi 2.1 Based on the high entropy alloy system, further improving its comprehensive mechanical properties will hopefully enable it to meet the application requirements of waste incineration boilers. Summary of the invention

[0007] In order to overcome the above-mentioned shortcomings of the prior art, the present invention is based on AlCoCrFeNi 2.1On the basis of the high entropy alloy system, the Mo element is further introduced to improve its high temperature stability and acid corrosion resistance, and the V element is introduced to refine the grains, reduce its thermal sensitivity, and improve wear resistance. By combining simple cold deformation and heat treatment processes, an alloy material with excellent comprehensive mechanical properties is obtained.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] The first aspect of the present invention provides a high-strength, tough and corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with a precipitation phase strengthening effect. The AlCoCrFeNiMoV high-entropy alloy comprises, by mass percentage, Al: 4.0-6.0%, Co: 18.0-20.0%, Cr: 15-17%, Fe: 17.0-19.0%, Ni: 37.0-39.0%, Mo: 2.0%-3.0%, and V: 0.5%-0.7%.

[0010] Preferably, the AlCoCrFeNiMoV high entropy alloy is Al4Co 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 High entropy alloy or Al6Co 18.5 Cr 16 Fe 19 Ni 38 Mo2V 0.5 High entropy alloy.

[0011] The second aspect of the present invention provides a method for preparing the high-strength, high-toughness, high-corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect as described in the first aspect, the method comprising the following steps:

[0012] S1. Weigh Al, Co, Cr, Fe, Ni, Mo, and V metal single substance raw materials according to the ratio of AlCoCrFeNiMoV high entropy alloy, and melt and cast them into ingots;

[0013] S2, performing a solution heat treatment on the ingot described in S1 to obtain a single-phase alloy ingot having a face-centered cubic (FCC) structure;

[0014] S3, performing cold deformation rolling with a deformation amount of 72-90% on the ingot after the solution heat treatment, so as to roll it into a plate;

[0015] S4. Perform annealing heat treatment on the rolled plate to obtain AlCoCrFeNiMoV high entropy alloy.

[0016] The high-strength, toughness and corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect provided by the present invention is precisely designed for complex AlCoCrFeNiMoV alloy. The Mo element is a refractory element with a melting point of up to 2896°C and is often used as a strengthening element for high-temperature alloys. Due to its large atomic radius, the introduction of the Mo element will cause significant distortion of the lattice, and with the increase of the Mo element content, a σ phase rich in (Cr, Mo) will be formed in the AlCoCrFeMoxNi alloy, thereby improving the hardness and strength of the cast alloy; and the V element also has a large atomic radius. After solution treatment, the performance of the cast alloy reaches the best comprehensive performance. After further cold rolling deformation with a huge deformation amount and annealing and recrystallization heat treatment, the FCC single-phase high-entropy alloy can be precipitated at high temperature through solid solution to precipitate a high-density strengthening phase precipitation phase, and then obtain a fine-scale precipitation phase heterogeneous structure in the matrix phase, and finally obtain an excellent alloy material that takes both plasticity and strength into consideration.

[0017] The present invention reasonably designs the composition and process of the AlCoCrFeNiMoV high entropy alloy to regulate the precipitation of high-density precipitation phases, thereby obtaining an alloy material with excellent comprehensive mechanical properties and high corrosion resistance, that is, high strength (yield strength is not less than 1100MPa, tensile strength is not less than 1300MPa), high plasticity (elongation ≥10%), and excellent corrosion resistance (self-corrosion voltage in 3.5% NaCl solution exceeds -0.41V, and self-corrosion current density is less than 1.82×10 -6 A / cm 2 ), so that it can be used to prepare the inner wall material of the waste incineration boiler. And this process is simple and easy to implement, which has a great promoting effect on large-scale production.

[0018] Preferably, in the metal single substance raw materials in step S1, the purity of Al, Co, Ni, Mo, and V is above 99.9wt%, and the purity of Cr and Fe is above 99.5wt%.

[0019] Preferably, the temperature of the solution heat treatment in step S2 is 900-1100° C., the holding time is 4-16 hours, and the steel is quenched to room temperature after the holding is completed.

[0020] Preferably, the cold deformation rolling in S3 is performed three times, and the average reduction ratio of each pass is 24% to 30%.

[0021] Preferably, the temperature of the annealing heat treatment in step S4 is 800-900° C., the holding time is 0.5-2 h, and the alloy is cooled to room temperature with the furnace after the holding is completed; after the annealing heat treatment, a face-centered cubic (FCC) nano-precipitate phase appears in the B2 matrix of the alloy.

[0022] Preferably, step S1 is to melt and cast into an ingot by a vacuum induction furnace.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention discloses a high-strength, tough, and corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with a precipitation phase strengthening effect and a preparation method thereof. The mass percentage of each element in the high-entropy alloy is Al: 4.0-6.0%, Co: 18.0-20.0%, Cr: 15-17%, Fe: 17.0-19.0%, Ni: 37.0-39.0%, Mo: 2.0%-3.0%, and V: 0.5%-0.7%. The present invention reasonably regulates the alloy composition and combines ingot solution heat treatment, cold rolling, and recrystallization heat treatment to prepare a dual-phase FCC+B2 lamellar composite material with excellent performance, i.e., a precipitation phase strengthened high-strength, tough, and corrosion-resistant alloy. The present invention designs nanoscale precipitation phase strengthening in the FCC single-phase high-entropy alloy, so that the alloy has a higher yield strength and tensile strength at room temperature without reducing the excellent plasticity, and the corrosion resistance is also significantly improved. The research found that the AlCoCrFeNiMoV high entropy alloy prepared by the present invention has high strength (yield strength not less than 1100MPa, tensile strength not less than 1300MPa), sufficient safety in use (elongation ≥10%), and excellent corrosion resistance (self-corrosion voltage in 3.5% NaCl solution exceeds -0.41V, and self-corrosion current density is less than 1.82×10 -6 A / cm 2 ). Therefore, the high entropy alloy of the present invention has excellent yield strength and tensile strength while maintaining high plasticity through the strengthening effect of the precipitated phase, and has high acid corrosion resistance, so that it can be used to prepare the inner wall material of the waste incineration boiler. In addition, the process scheme of the present invention is simple and easy to implement, which has a great promoting effect on large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 XRD pattern of the AlCoCrFeNiMoV high entropy alloy of Example 1;

[0026] Figure 2 This is a scanning electron microscope photograph of the AlCoCrFeNiMoV high entropy alloy of Example 1;

[0027] Figure 3 is a tensile stress-strain diagram of the AlCoCrFeNiMoV high entropy alloy of Example 1 at room temperature;

[0028] Figure 4 is a tensile stress-strain diagram of the AlCoCrFeNiMoV high entropy alloy of Example 2 at room temperature;

[0029] Figure 5 This is a tensile fracture diagram of the AlCoCrFeNiMoV high entropy alloy of Example 1 at room temperature;

[0030] Figure 6 This is a tensile fracture diagram of the AlCoCrFeNiMoV high entropy alloy of Example 2 at room temperature;

[0031] Figure 7 is a polarization curve diagram of the AlCoCrFeNiMoV high entropy alloy of Example 1 in a 3.5% NaCl solution;

[0032] Figure 8 is a polarization curve diagram of the AlCoCrFeNiMoV high entropy alloy of Example 2 in a 3.5% NaCl solution;

[0033] Fig. 9 Al4Co without solution treatment 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 Tensile stress-strain diagram of a high entropy alloy at room temperature. DETAILED DESCRIPTION

[0034] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0035] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0036] In the metal single substance raw materials involved in the following embodiments or comparative examples, the purity of Al, Co, Ni, Mo, and V is above 99.9wt%, and the purity of Cr and Fe is above 99.5wt%.

[0037] Example 1: Al4Co 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 High entropy alloy and preparation method thereof

[0038] (1) By mass percentage, the configuration composition is Al4Co 20 Cr16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 The alloy is melted and cast into ingots in a vacuum induction furnace;

[0039] (2) subjecting the ingot of step (1) to a solution heat treatment, i.e., subjecting the ingot to a temperature of 1000° C. for 12 h, and then quenching the ingot to room temperature to obtain a single-phase alloy ingot having a face-centered cubic (FCC) structure;

[0040] (3) cold deformation rolling (cold rolling) is performed on the alloy ingot after the solution heat treatment, so that the deformation amount is 80%, and then rolled into a plate;

[0041] (4) The cold-deformed parts are subjected to annealing heat treatment, that is, they are kept at 850°C for 1 hour, and then cooled to room temperature in the furnace after the end of the heat preservation, and finally a high-entropy alloy with good comprehensive properties is obtained.

[0042] Figure 1 Al4Co prepared in Example 1 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 XRD spectrum of high entropy alloy. It can be seen from the figure that the alloy is composed of FCC phase and B2 phase.

[0043] Figure 2 Al4Co prepared in Example 1 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 Microstructure photos of high entropy alloys show that Al4Co 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 The alloy structure of high entropy alloy is a lamellar structure composed of irregular FCC phase and B2 phase, and a large number of nano-scale precipitation phases are distributed in the matrix structure. At the same time, due to the solution heat treatment, dense dark granular precipitation phases appear in the light-colored matrix. This is because a large amount of alloy elements are dissolved in the solid solution at high temperature to form a supersaturated state. During the cooling process, the solute atoms in the supersaturated solid solution gradually precipitate, thereby forming fine precipitation phases.

[0044] Take 10 -3 The alloy sample was stretched at a stretching rate of mm / s. Figure 3As shown. It can be seen that at room temperature, the sample elongation reaches 10%, the yield strength reaches 1642MPa, and there is obvious strain hardening behavior during deformation, and the tensile strength is 1766MPa. 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 A high entropy alloy [i.e., a high entropy alloy prepared using only steps (1), (3), and (4)] was used as a control to test its tensile stress-strain at room temperature. Fig. 9 It can be seen that its tensile strength is only about 1600MPa. Figure 3 It can be seen that the Al4Co prepared by solution treatment in this application 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 High entropy alloys have a precipitation strengthening effect, which can increase their strength to nearly 1800MPa.

[0045] Figure 5 This is a tensile fracture diagram at room temperature of the high-strength, high-toughness, high-corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect obtained in Example 1. The tensile fracture surface shows that the high-entropy alloy has a ductile fracture with dimple characteristics. Although it also has a smooth surface of cleavage brittle fracture, ductile fracture is the main effect.

[0046] Figure 7 The polarization curve of the high-strength, high-toughness, high-corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect prepared in Example 1 is -0.429 V in a 3.5% NaCl solution, and the self-corrosion current density is 1.1691×10 -7 A / cm 2 , while the self-corrosion current of super austenitic stainless steel S32654, which is commonly used as a material for waste incineration boilers, is 6.89×10 -6 A / cm 2 It can be seen that the high-strength, toughness and corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect prepared in Example 1 has better corrosion resistance than super austenitic stainless steel S32654.

[0047] Example 2: Al6Co 18.5 Cr 16 Fe 19 Ni 38 Mo2V 0.5 High entropy alloy and preparation method thereof

[0048] (1) By mass percentage, the configuration composition is Al6-Co 18.5 -Cr 16 -Fe 19 -Ni 38 -Mo2-V 0.5 The alloy is melted and cast into ingots in a vacuum induction furnace;

[0049] (2) subjecting the ingot of step (1) to a solution heat treatment, i.e., placing the ingot at 1000° C. for 12 h, and then quenching the ingot to room temperature to obtain a single-phase alloy ingot having a face-centered cubic (FCC) structure;

[0050] (3) cold deformation rolling (cold rolling) is performed on the alloy ingot after the solution heat treatment, so that the deformation amount is 80%, and then rolled into a plate;

[0051] (4) The cold-deformed parts are subjected to annealing heat treatment, that is, they are kept at 850°C for 1 hour, and then cooled to room temperature in the furnace after the end of the heat preservation, and finally a high-entropy alloy with good comprehensive properties is obtained.

[0052] Take 10 -3 The alloy sample was stretched at a stretching rate of mm / s. Figure 4 As shown, it can be seen that at room temperature, the elongation of the sample reaches 23%, the yield strength reaches 1100 MPa, and there is obvious strain hardening behavior during the deformation process, and the tensile strength is 1305 MPa.

[0053] Figure 6 This is a tensile fracture diagram of the AlCoCrFeNiMoV high entropy alloy prepared in Example 2 at room temperature. The tensile fracture surface shows that it is almost entirely ductile fracture with dimple characteristics, which is consistent with the ultra-high plasticity in the tensile stress-strain diagram.

[0054] Figure 8 The polarization curve of the AlCoCrFeNiMoV high entropy alloy prepared in Example 2 is shown in Figure 2. It can be seen that the self-corrosion voltage of the high entropy alloy in 3.5% NaCl solution is -0.405 V, and the self-corrosion current density is 1.8115×10 -6 A / cm 2 .

[0055] Comparative Example 1: Al9Co 19.6 Cr 17.3 Fe 18.6 Ni 19.5 Mo 16 High entropy alloy and preparation method thereof

[0056] (1) By mass percentage, the configuration composition is Al9Co 19.6 Cr 17.3Fe 18.6 Ni 19.5 Mo 16 The alloy is melted and cast into an ingot by a vacuum induction furnace to obtain a single-phase alloy ingot with a body-centered cubic (BCC) structure;

[0057] (2) subjecting the ingot of step (1) to a solution heat treatment, i.e., subjecting the ingot to a temperature of 1000° C. for 12 h, and then quenching the ingot to room temperature to obtain a single-phase alloy ingot having a face-centered cubic (FCC) structure;

[0058] (3) cold deformation rolling (cold rolling) is performed on the alloy ingot after the solution heat treatment, so that the deformation amount is 80%, and then rolled into a plate;

[0059] (4) The cold-deformed parts are subjected to annealing heat treatment, that is, they are kept at 850°C for 1 hour and then cooled to room temperature in the furnace.

[0060] The high entropy alloy has no yield stage at room temperature, a fracture strength of 900 MPa, and a plasticity of only 6%. The tensile strength of Example 1 is relatively high (yield strength reaches 1642 MPa), and the yield strength of Example 2 reaches 1100 MPa, and the elongation reaches 23%. At the same time, the self-corrosion current density in 3.5% NaCl solution is 2.250×10 -6 A / cm 2 , which is greater than the high entropy alloys prepared in Example 1 and Example 2, indicating that adding Mo and V elements simultaneously in Example 1 and Example 2 not only improves the corrosion resistance of the high entropy alloy compared to adding only Mo element, but also has higher strength and toughness under tensile conditions. 9.6 Co 20.8 Cr 18.4 Fe 19.7 Ni 20.7 V 10.8 High entropy alloy and preparation method thereof

[0061] (1) Configuration composition is Al 9.6 Co 20.8 Cr 18.4 Fe 19.7 Ni 20.7 V 10.8 The alloy is melted and cast into an ingot by a vacuum arc furnace to obtain a single-phase alloy ingot with a body-centered cubic (BCC) structure;

[0062] (2) subjecting the ingot of step (1) to a solution heat treatment, i.e., subjecting the ingot to a temperature of 1000° C. for 12 h, and then quenching the ingot to room temperature to obtain a single-phase alloy ingot having a face-centered cubic (FCC) structure;

[0063] (3) cold deformation rolling (cold rolling) is performed on the alloy ingot after the solution heat treatment, so that the deformation amount is 80%, and then rolled into a plate;

[0064] (4) The cold-deformed parts are subjected to annealing heat treatment, that is, they are kept at 850°C for 1 hour and then cooled to room temperature in the furnace.

[0065] At room temperature, there is no yield stage, the fracture strength is only 900MPa and the plasticity is only 6%, while the high entropy alloy prepared in Example 1 has a yield strength of more than 1600MPa and a plasticity of more than 10%, and the high entropy alloy prepared in Example 2 has a yield strength of 1100MPa and a plasticity of more than 23%, indicating that the addition of Mo and V elements at the same time improves the strength and toughness of the high entropy alloy and improves the mechanical properties compared to adding only V elements. At the same time, the self-corrosion current density of Comparative Example 2 in 3.5% NaCl solution is 2.527A / cm 2 , which is greater than the high entropy alloys prepared in Examples 1 and 2, further confirming that the simultaneous addition of Mo and V elements improves the corrosion resistance of the high entropy alloy.

[0066] In summary, the present invention provides an AlCoCrFeNiMoV high entropy alloy with excellent comprehensive mechanical properties, high strength (yield strength not less than 1100MPa, tensile strength not less than 1300MPa), sufficient safety in use (elongation ≥10%), and excellent corrosion resistance (self-corrosion voltage in 3.5% NaCl solution can exceed -0.41V, self-corrosion current density is less than 1.82×10 -6 A / cm 2 ).

[0067] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A high-strength, high-toughness, high-corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect, characterized in that: Calculated by mass percentage, the AlCoCrFeNiMoV high entropy alloy includes Al: 4.0-6.0%, Co: 18.0-20.0%, Cr: 15-17%, Fe: 17.0-19.0%, Ni: 37.0-39.0%, Mo: 2.0%-3.0%, and V: 0.5%-0.7%.

2. The high-strength, toughness, and corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect according to claim 1, characterized in that: The AlCoCrFeNiMoV high entropy alloy is Al4Co 20 Cr 16.8 Fe 18.2 Ni 38 Mo 2.5 V 0.5 High entropy alloy or Al6Co 18.5 Cr 16 Fe 19 Ni 38 Mo2V 0.5 High entropy alloy.

3. The method for preparing the high-strength, toughness, and corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect according to claim 1 or 2, characterized in that: The following steps are involved: S1. Weighing Al, Co, Cr, Fe, Ni, Mo, and V metal raw materials according to the ratio of AlCoCrFeNiMoV high entropy alloy and melting and casting them into ingots; S2. performing a solution heat treatment on the ingot described in S1 to obtain a single-phase alloy ingot having a face-centered cubic (FCC) structure; S3, performing cold deformation rolling with a deformation amount of 72-90% on the ingot after the solution heat treatment, so as to roll it into a plate; S4. Performing annealing heat treatment on the rolled plate to obtain an AlCoCrFeNiMoV high entropy alloy.

4. The method for preparing a high-strength, high-toughness, high-corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect according to claim 3, characterized in that: In the metal element raw materials of step S1, the purity of Al, Co, Ni, Mo, and V is above 99.9 wt%, and the purity of Cr and Fe is above 99.5 wt%.

5. The method for preparing a high-strength, high-toughness, high-corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect according to claim 3, characterized in that: The temperature of the solution heat treatment in step S2 is 900-1100° C., the holding time is 4-16 hours, and the steel is quenched to room temperature after the holding is completed.

6. The method for preparing a high-strength, high-toughness, high-corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect according to claim 3, characterized in that: The cold deformation rolling in S3 is performed three times, and the average reduction rate of each pass is 24% to 30%.

7. The method for preparing a high-strength, high-toughness, high-corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect according to claim 3, characterized in that: The annealing heat treatment temperature in step S4 is 800-900° C., the holding time is 0.5-2 hours, and the alloy is cooled to room temperature in the furnace after the holding period. After the annealing heat treatment, a face-centered cubic (FCC) nano-precipitate phase appears in the B2 matrix of the alloy.

8. The method for preparing a high-strength, toughness, and corrosion-resistant AlCoCrFeNiMoV high-entropy alloy with precipitation phase strengthening effect according to claim 3, characterized in that: Step S1 is to melt and cast into an ingot in a vacuum induction furnace.

Citation Information

Cited By

  • Necklace-shaped heterostructure high-entropy alloy and preparation method thereof

    CN119776711A