ITO film preparation method and ITO film

By using low-density ITO ingots in the preparation of ITO films and premelting, preliminary heating and sufficient preheating in the cavity of the evaporation equipment, combined with appropriate evaporation parameter settings, the rough appearance and transmittance of the film in the preparation of ITO films is solved. The problem of low is that ITO film preparation with uniform membrane quality and high transmittance is achieved.

CN118932285APending Publication Date: 2024-11-12JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411132740.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The problem of rough appearance and low transmittance caused by the ITO film preparation method in the prior art.

Method used

The electron beam evaporation is carried out by using low-density ITO ingots to perform electron beam evaporation, and the temperature of the evaporation equipment is adjusted by premelting, initial heating and sufficient preheating to the set current value, and cooling the air break after the evaporation is completed. , current, oxygen flow and rotation speed parameters are used to prepare a uniform ITO film.

Benefits of technology

The ITO film has uniform film quality and high transmittance, and solved the problem of rough appearance and low transmittance of the film. The ITO film after evaporation can reach 97%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932285A_ABST
    Figure CN118932285A_ABST
Patent Text Reader

Abstract

The invention provides an LED (Light Emitting Diode) preparation method and an ITO (Indium Tin Oxide) film. The method comprises the following steps: providing a low-density ITO ingot; the low-density ITO ingot is placed in a cavity of evaporation equipment, and the cavity of the evaporation equipment is adjusted to a set state; in the cavity of the evaporation equipment, the low-density ITO ingot is sequentially pre-melted, preliminarily heated and fully preheated to a set evaporation current value; and carrying out evaporation on the low-density ITO ingot through the set current value, and after the evaporation is completed, carrying out cooling and gas breaking to obtain the ITO film. The problems that an ITO film prepared by an ITO film preparation method in the prior art is rough in appearance and low in transmittance are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductors, and in particular to an ITO film preparation method and the ITO film. Background Art

[0002] ITO film is an n-type semiconductor material with high conductivity, high visible light transmittance, high mechanical hardness and good chemical stability. It is the most commonly used film material for transparent electrodes of liquid crystal displays (LCDs), plasma displays (PDPs), electroluminescent displays (EL / OLEDs), touch panels, solar cells and other electronic instruments.

[0003] At present, the ITO film deposited by electron beam evaporation has a rough appearance and low transmittance, which fails to meet the current performance requirements. Summary of the invention

[0004] Based on this, the purpose of the present invention is to provide an ITO film preparation method and an ITO film, aiming to solve the problem that the ITO film prepared by the ITO film preparation method in the prior art has a rough appearance and low transmittance.

[0005] The embodiment of the present invention is implemented as follows: In one aspect, the present invention provides a method for preparing an ITO thin film, the method comprising: Providing a low-density ITO ingot; Placing the low-density ITO ingot in a cavity of an evaporation device, and adjusting the cavity of the evaporation device to a set state; In the chamber of the evaporation equipment, the low-density ITO ingot is pre-melted, preliminarily heated, and fully preheated to a set evaporation current value in sequence; The low-density ITO ingot is evaporated by the set current value, and after the evaporation is completed, it is cooled and degassed to obtain an ITO film.

[0006] Furthermore, in the above-mentioned ITO thin film preparation method, the low-density ITO ingot comprises the following components by mass percentage: SnO2: 5%~10%, the balance is In203.

[0007] Furthermore, in the above-mentioned ITO thin film preparation method, the size of the low-density ITO ingot is 25mm*10mm.

[0008] Furthermore, in the above-mentioned ITO thin film preparation method, the setting state includes: The temperature is set to 300℃~330℃, and the temperature duration is greater than 30min.

[0009] Furthermore, in the above-mentioned ITO thin film preparation method, the setting state further comprises: The electron gun spot scanning size is 60% to 80% of the area of ​​the low-density ITO ingot, and the current is less than 6 mA. Furthermore, in the above-mentioned ITO thin film preparation method, the setting state further comprises: The plating pot speed is set to 8r / min~10r / min. Furthermore, in the above-mentioned ITO thin film preparation method, the setting state further comprises: 10~12sccm of oxygen is introduced and the stabilization time is more than 60S.

[0010] Furthermore, in the above-mentioned ITO thin film preparation method, the steps of pre-melting, preliminarily heating and fully preheating the low-density ITO ingot to a set evaporation current value in the cavity of the evaporation equipment in sequence include: In a first preset time, the evaporation current is gradually and evenly increased from 0 to a first preset current value and maintained for a preset time, so that the ITO ingot is initially heated; In a second preset time, gradually and evenly increase the current from the first preset current value to a second preset current value and maintain the current for a set time, so that the ITO ingot is fully preheated; Within a third preset time, the current is gradually and evenly reduced from the second preset current value to a third preset current and maintained for a set time to reach the current value required for evaporation.

[0011] Furthermore, in the above-mentioned ITO film preparation method, the cooling time is 20 minutes to 40 minutes, and the cooling temperature is 120°C to 180°C.

[0012] In another aspect, the present invention provides an ITO film, which is prepared by any of the above-mentioned ITO film preparation methods.

[0013] The present invention provides a low-density ITO ingot; places the low-density ITO ingot in a cavity of an evaporation device, and adjusts the cavity of the evaporation device to a set state; in the cavity of the evaporation device, sequentially pre-melts the low-density ITO ingot, preliminarily heats it, and fully preheats it to a set evaporation current value; evaporates the low-density ITO ingot at the set current value, and cools and degasses it after the evaporation is completed to obtain an ITO film. The obtained film has uniform quality and high transmittance, and solves the problem that the film prepared by the ITO film preparation method in the prior art has a rough appearance and low transmittance. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a flow chart of a method for preparing an ITO thin film according to an embodiment of the present invention; Figure 2It is a structural schematic diagram of a cavity of an evaporation device in a method for preparing an ITO thin film in one embodiment of the present invention; The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0015] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0016] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.

[0017] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0018] The embodiment of the present invention aims at the problem that the ITO film prepared in the prior art has a rough appearance and low transmittance, and proposes a method for preparing an ITO film and an ITO film.

[0019] See also Figure 1 , which is a flow chart of the ITO thin film preparation method of the present invention, and the ITO thin film preparation method includes steps S10~S13.

[0020] Step S10, providing a low-density ITO ingot.

[0021] Among them, in the embodiment of the present invention, the mass percentage of the raw material used for preparing the ITO film is SnO2: 5%~10%, and the balance is In203. A low-density ITO ingot is used, and the size is 25mm (φ)*10mm (h).

[0022] Step S11, placing the low-density ITO ingot in a cavity of an evaporation device, and adjusting the cavity of the evaporation device to a set state.

[0023] In order to ensure the quality of evaporation, the cavity of the evaporation equipment used for evaporation is adjusted to a set state before evaporation. Specifically, in the embodiment of the present invention, the evaporation equipment is an electron beam evaporation equipment, which uses an electron gun to generate and focus a high-energy electron beam, such as Figure 2 As shown, exemplarily, in order to realize thin film evaporation, a base for fixing the substrate, a crucible for carrying the material to be evaporated, a heating source and a ventilation pump are also provided in the cavity of the evaporation equipment.

[0024] More specifically, the setting state in the chamber includes multiple states, among which the main one is that the vacuum in the chamber needs to be evacuated to below 3.0E-6 before evaporation, so that the air (impurity gas) in the chamber is in a very small state, otherwise the evaporation process will affect the oxygen concentration in the chamber; The cavity temperature is set at 300℃~330℃. The overall cavity temperature can be kept uniform by adjusting the angle of the heating source (quartz heating lamp). This is conducive to uniform heating of the base layer, and the temperature needs to be maintained for more than 30 minutes to improve the ITO adhesion ability during the ITO evaporation process.

[0025] The scanning size of the electron gun spot is 60%~80% of the ITO ingot area, so that the ITO ingot can be fully utilized and the waste of ITO ingot can be avoided (it is changed every furnace, because the oxygen content and humidity of the target material change greatly after the evaporation cavity is broken). The machine voltage is fixed (commonly 6000V), and the current is controlled below 6mA. Among them, the current is mainly used to drive the electron gun to generate an electron beam. The current size can be controlled by controlling the cooling water temperature or flow. Minimizing the current is conducive to the overall temperature of the target material being relatively uniform after heating, so that the mobility of ITO can be higher and relatively stable; The plating pot speed is set to 8r / min~10r / min, which is conducive to uniform heating of the base layer and can make the ITO film thickness more uniform. The uniformity of the film thickness can be controlled within 5%; 10~12sccm of oxygen (purity 5N or above) is introduced, and the stabilization time is more than 60S. At this time, the overall chamber is about 1.0E-4~3.0E-4. The above steps are the key to controlling the oxygen partial pressure. Controlling the oxygen partial pressure can control the oxidation degree of ITO, improve the mobility of ITO, and make the ITO film more uniform.

[0026] Step S12, in the chamber of the evaporation equipment, sequentially pre-melting, preliminarily heating and fully pre-heating the low-density ITO ingot to a set evaporation current value.

[0027] Wherein, within a first preset time, the evaporation current is gradually and evenly increased from 0 to a first preset current value and maintained for a set time, so that the ITO ingot is initially heated; In the second preset time, the current is gradually and evenly increased from the first preset current value to the second preset current value and maintained for the set time, so that the ITO ingot is fully preheated; In a third preset time, the current is gradually and evenly reduced from the second preset current value to the third preset current and maintained for a set time to reach the current value required for evaporation; Specifically, the ITO ingot is pre-melted in the early stage. The first step is to increase the current from 0 to 2mA evenly within 20S and keep it for 2 minutes to preliminarily heat the ITO ingot. The second step is to increase the current from 2 to 6.5mA evenly within 60S and keep it for 2 minutes to fully preheat the ITO ingot. The third step is to reduce the current from 6.5 to 5.5mA evenly within 10S and keep it for 1 minute to reach the current value during evaporation. This power corresponds to an ITO plating rate of 1Å / S. At this time, open the electron gun shield to start evaporation.

[0028] Step S13, vapor-depositing the low-density ITO ingot by using the set current value, and cooling and degassing after the vapor-deposition is completed to obtain an ITO film.

[0029] Among them, in this embodiment, the thickness is set to 2500±100Å. After the evaporation is completed, the cavity is cooled for 20min~40min, for example, 30 minutes, and the temperature is reduced by 120℃~180℃, for example, around 150℃, and the vacuum is broken. Breaking the vacuum at too high a temperature will accelerate the aging of the cavity accessories, and will also make it more likely to cause the substrate and quartz heating lamp to drop in temperature and crack. After the evaporation is completed, the transmittance of the ITO film can reach 97%.

[0030] In addition, the present invention also provides an ITO film, which is prepared by the above-mentioned ITO film preparation method.

[0031] In summary, the ITO film preparation method and ITO film proposed in the embodiments of the present invention provide a low-density ITO ingot; place the low-density ITO ingot in the cavity of the evaporation equipment, and adjust the cavity of the evaporation equipment to a set state; in the cavity of the evaporation equipment, pre-melt the low-density ITO ingot, preliminarily heat it, and fully preheat it to the set evaporation current value in sequence; evaporate the low-density ITO ingot at the set current value, and cool and degas after the evaporation is completed to obtain an ITO film. The obtained film has uniform quality and high transmittance, which solves the problem of rough appearance and low transmittance of the film prepared by the ITO film preparation method in the prior art.

[0032] Embodiment 1 Embodiment 1 of the present invention provides a method for preparing an ITO thin film, comprising: Use a low-density ITO ingot with a mass percentage of In203:SnO28% of ITO raw materials and a size of 25mm (φ) * 10mm (h); Before evaporation, the vacuum needs to be pumped to below 3.0E-6 to keep the air (impurity gas) in the cavity in a very small state; The cavity temperature was set to 320°C; The electron gun spot scanning size is 70% of the ITO ingot area, the machine voltage is fixed at 6000V, and the current is controlled below 6mA; The plating pot speed is set to 8r / min; 6sccm of oxygen (purity 5N or above) is introduced, and the stabilization time is more than 60S; The ITO ingot is pre-melted in the early stage. The first step is to increase the current from 0 to 2mA evenly within 20S and keep it for 2 minutes to preheat the ITO ingot. The second step is to increase the current from 2 to 6.5mA evenly within 60S and keep it for 2 minutes to fully preheat the ITO ingot. The third step is to reduce the current from 6.5 to 5.5mA evenly within 10S and keep it for 1 minute to reach the current value during evaporation. This power corresponds to an ITO plating rate of 1Å / S. At this time, open the electron gun shield to start evaporation; The thickness was set to 2500. After the evaporation was completed, the chamber was cooled for 30 minutes, the temperature dropped to 150°C, and the vacuum was broken. The ITO evaporation is completed to obtain an ITO thin film.

[0033] Embodiment 2 The second embodiment of the present invention also provides a method for preparing an ITO thin film. The difference between the method for preparing the thin film in this embodiment and the method for preparing the thin film in the first embodiment is that: 8 sccm of oxygen was introduced.

[0034] Embodiment 3 Embodiment 3 of the present invention also provides a thin film preparation method. The difference between the thin film preparation method in this embodiment and the thin film preparation method in embodiment 1 is that: 10 sccm of oxygen was introduced.

[0035] Embodiment 4 The fourth embodiment of the present invention also provides a thin film preparation method. The difference between the thin film preparation method in this embodiment and the thin film preparation method in the first embodiment is that: 12 sccm of oxygen was introduced.

[0036] Embodiment 5 Embodiment 5 of the present invention also provides a thin film preparation method. The difference between the thin film preparation method in this embodiment and the thin film preparation method in embodiment 1 is that: 14 sccm of oxygen was introduced.

[0037] Embodiment 6 Embodiment 6 of the present invention also provides a thin film preparation method. The difference between the thin film preparation method in this embodiment and the thin film preparation method in embodiment 1 is that: 16 sccm of oxygen was introduced.

[0038] Please refer to Table 1 below, which shows the corresponding parameters of the above-mentioned Embodiments 1 to 6 of the present invention and the corresponding properties of the ITO films deposited therefrom.

[0039] Table 1

[0040] It can be clearly seen that by providing a low-density ITO ingot; placing the low-density ITO ingot in the cavity of the evaporation equipment, and adjusting the cavity of the evaporation equipment to a set state; in the cavity of the evaporation equipment, the low-density ITO ingot is pre-melted, preliminarily heated, and fully preheated to the set evaporation current value in sequence; the low-density ITO ingot is evaporated by the set current value, and after the evaporation is completed, the ITO thin film is obtained by cooling and degassing. The obtained film has uniform quality and high transmittance, which solves the problem of rough appearance and low transmittance of the film prepared by the ITO thin film preparation method in the prior art.

[0041] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing an ITO thin film, characterized in that: The method comprises: Providing a low-density ITO ingot; Placing the low-density ITO ingot in a cavity of an evaporation device, and adjusting the cavity of the evaporation device to a set state; In the chamber of the evaporation equipment, the low-density ITO ingot is pre-melted, preliminarily heated, and fully preheated to a set evaporation current value in sequence; The low-density ITO ingot is evaporated by the set current value, and after the evaporation is completed, it is cooled and degassed to obtain an ITO film.

2. The ITO film preparation method according to claim 1, characterized in that: The low-density ITO ingot comprises the following components by mass percentage: SnO2: 5%~10%, the balance is In203.

3. The ITO film preparation method according to claim 1, characterized in that: The size of the low-density ITO ingot is 25 mm*10 mm.

4. The ITO film preparation method according to claim 1, characterized in that: The setting state includes: The temperature is set to 300℃~330℃, and the temperature duration is greater than 30min.

5. The ITO film preparation method according to claim 4, characterized in that: The setting state also includes: The electron gun spot scanning size is 60% to 80% of the area of ​​the low-density ITO ingot, and the current is less than 6 mA.

6. The method for preparing an ITO film according to claim 5, wherein: The setting state also includes: The plating pot speed is set to 8r / min~10r / min.

7. The method for preparing an ITO film according to claim 6, wherein: The setting state also includes: 10~12sccm of oxygen is introduced and the stabilization time is more than 60S.

8. The method for preparing an ITO film according to claim 1, wherein: The steps of pre-melting, preliminarily heating, and fully preheating the low-density ITO ingot to a set evaporation current value in the cavity of the evaporation equipment in sequence include: In a first preset time, the evaporation current is gradually and evenly increased from 0 to a first preset current value and maintained for a preset time, so that the ITO ingot is initially heated; In a second preset time, gradually and evenly increase the current from the first preset current value to a second preset current value and maintain the current for a set time, so that the ITO ingot is fully preheated; Within a third preset time, the current is gradually and evenly reduced from the second preset current value to a third preset current and maintained for a set time to reach the current value required for evaporation.

9. The method for preparing an ITO film according to claim 1, wherein: The cooling time is 20 min to 40 min, and the cooling temperature is 120° C. to 180° C.

10. An ITO film, characterized in that: The ITO film is prepared by the ITO film preparation method according to any one of claims 1 to 9.