Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material and preparation method thereof
By growing TiO2 nanotubes in situ on the surface of Ti sheet and electrodepositing Cu-RuO2 catalytic layer, Cu-RuO2/TiO2 nanotubes/Ti anode material was prepared, which solved the problem of insufficient catalytic activity and stability of traditional electrode materials, and achieved the Highly efficient chlorine-oxygen potential difference and electrocatalytic performance, suitable for low energy consumption and low cost requirements of the chlor-alkali industry.
Patent Information
- Application Number
- CN202411106327.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The catalytic activity and stability of the anode material of electrolyzed sodium chloride solution in the existing chlor-alkali industry is insufficient, resulting in high energy consumption and high cost. The electrodes synthesized by traditional thermal decomposition methods are prone to cracking, making it difficult to meet the needs of industrial production.
TiO2 nanotubes were grown in situ on the surface of Ti sheet by anodic oxidation, and Cu-RuO2 catalytic coating was prepared on its surface by electrodeposition method to form Cu-RuO2/TiO2 Nanotube/Ti chloro-excited anode material avoids the coating-sintering process and improves catalytic activity and stability.
The Cu-RuO2/TiO2 nanotube/Ti anode material obtained by this method has high catalytic activity and high chlorine-oxygen potential difference, small charge transfer resistance, significantly improving the selectivity of chlorine analysis potential and electrocatalytic performance, and reducing commercial DSA electrodes chlorine potential is suitable for industrial production.
Smart Images

Figure CN118932400A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrode material preparation, and specifically relates to Cu-RuO 2 / TiO 2 Preparation method of nanotube / Ti chlorine evolution anode material, also involving the Cu-RuO 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution. Background Art
[0002] As an important part of the modern chemical industry, the chlor-alkali industry has caustic soda (sodium hydroxide), hydrogen and chlorine as its main products. It has high economic value and is widely used in various sectors of the national economy, such as papermaking, textiles, petroleum, light industry, and food processing. However, the current electricity consumption of chlor-alkali production accounts for about 10% of the total electricity consumption of the entire chemical industry. The power supply and electricity price have a great impact on the cost of the chlor-alkali industry. The key link of the chlor-alkali industry is electrolysis technology, in which the catalytic activity, stability, and selectivity of the anode material will directly affect the production efficiency, product quality, and cost of the chlor-alkali production process. Therefore, designing and preparing anode materials with excellent chlorine evolution performance is the key to reducing the energy consumption and cost of the chlor-alkali industry.
[0003] At present, the commercial electrodes for electrolyzing sodium chloride solution for chlorine evolution are mainly ruthenium-iridium-coated titanium anodes (DSA). During the electrolysis process, the catalytic coating is deactivated due to problems such as easy dissolution and peeling of the active components, causing electrode failure. At the same time, in addition to the chlorine evolution reaction, the anode is also accompanied by an oxygen evolution reaction. When the chlorine-oxygen potential difference is close, the selectivity of the electrode chlorine evolution reaction is significantly weakened, reducing its current efficiency. In addition, the precipitated oxygen will form bubbles on the electrode surface. The attachment and detachment of the bubbles will cause mechanical impact on the electrode surface, destroying the structure and stability of the electrode. Therefore, it is urgent to design and develop chlorine evolution anode materials with high catalytic activity, high chlorine-oxygen potential difference and high stability.
[0004] In recent years, researchers have found that by doping transition metal elements, building multilayer structures, introducing defects and other methods to regulate the electronic structure and active sites of chlorine evolution electrodes, their catalytic activity, stability and chlorine-oxygen potential difference can be further improved. 2 It can increase the number of electrons in the d-band center, weaken the binding strength with the oxygen evolution reaction intermediates, delay the kinetics of the oxygen evolution reaction, and thus improve the selectivity of the chlorine evolution reaction. 2 (denoted as Cu-RuO 2) The catalytic coating is beneficial to improving the chlorine evolution performance. However, the chlorine evolution electrode synthesized by the traditional thermal decomposition method is prone to surface catalyst particle agglomeration and coating cracking. Therefore, it is very necessary to design and develop a new process for preparing electrocatalytic chlorine evolution anode materials that is simple to operate and suitable for industrial production. Summary of the invention
[0005] The present invention aims to provide Cu-RuO 2 / TiO 2 The invention discloses a method for preparing a nanotube / Ti chlorine evolution anode material. The chlorine evolution anode material has high catalytic activity and high chlorine-oxygen potential difference.
[0006] Another object of the present invention is to provide Cu-RuO 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution.
[0007] The technical solution adopted by the present invention is that Cu-RuO 2 / TiO 2 The preparation method of nanotube / Ti chlorine evolution anode material is to use a mixed solution of ammonium fluoride, water and ethylene glycol as an electrolyte, and to in-situ grow TiO on the surface of a Ti sheet by an anodic oxidation method. 2 Nanotubes, and then the Cu-RuO with high catalytic activity can be prepared by electrodeposition. 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution.
[0008] The present invention is also characterized in that:
[0009] Follow the steps below to implement it:
[0010] Step 1, pretreatment of Ti sheet:
[0011] The Ti sheet was polished and cleaned with distilled water, then ultrasonically degreased and deoiled in a 0.01-1M sodium hydroxide solution, then placed in a 0.5-1.5M oxalic acid solution, and etched in a water bath for several hours to further remove the oxide layer. After cleaning, it was stored in ethanol for later use.
[0012] Step 2: In-situ growth of TiO on the surface of Ti sheet 2 Nanotubes:
[0013] A two-electrode system is used, with a mixture of ammonium fluoride, water and ethylene glycol as the electrolyte, the Ti sheet pretreated in step 1 as the anode and the Pt mesh as the cathode, the Ti sheet is subjected to anodization treatment, and finally the temperature is raised to 350-550°C in a muffle furnace at a rate of 1-10°C / min, kept at this temperature for 1-4h, and cooled naturally to obtain TiO 2 Nanotube / Ti electrode.
[0014] Step 3, Cu-RuO 2 / TiO 2 Preparation of nanotube / Ti chlorine evolution anode material:
[0015] The TiO prepared in step 2 2 The nanotube / Ti electrode is used as the cathode, the Pt mesh is used as the anode, and a mixed solution of ruthenium chloride, copper nitrate trihydrate, aminosulfonic acid, potassium chloride, hydrochloric acid, and water is used as the electrolyte for electrodeposition treatment. Finally, the temperature is raised to 350-550°C at a rate of 1-10°C / min in a muffle furnace, kept at this temperature for 1-4 hours, and cooled naturally to obtain Cu-RuO 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution.
[0016] In step 1, the water bath etching temperature is 70 to 90° C., and the etching time is 1 to 3 hours.
[0017] In step 2, the voltage of anodization is 30 to 90 V, and the time is 10 to 60 minutes.
[0018] In step 3, the current density of the electrodeposition is 5-20 mA / cm 2 , time is 5 to 30 minutes.
[0019] In step 3, in the electrolyte, the concentration of ruthenium chloride is 5-15 mM, the concentration of copper nitrate trihydrate is 0.05-5 mM, the concentration of aminosulfonic acid is 1-10 mM, the concentration of hydrochloric acid is 5-100 mM, and the concentration of potassium chloride is 0.05-1 M.
[0020] Another technical solution adopted by the present invention is that Cu-RuO 2 / TiO 2 The nanotube / Ti chlorine evolution anode material is prepared by the above method.
[0021] The beneficial effects of the present invention are:
[0022] (1) Cu-RuO prepared by the present invention 2 / TiO 2 Nanotube / Ti chlorine evolution anode material has the advantages of small charge transfer resistance and large chlorine-oxygen potential difference. 2 The chlorine evolution potential is only 1.081V (vs. SCE) at a current density of , which is 49mV lower than that of the commercial DSA electrode, showing excellent electrocatalytic chlorine evolution performance.
[0023] (2) The present invention firstly uses an anodic oxidation method to in-situ grow TiO on a Ti sheet. 2 The nanotubes were then electrodeposited onto TiO 2In situ preparation of Cu-doped RuO on the surface of nanotube / Ti sheet 2 Catalytic coating to obtain Cu-RuO 2 / TiO 2 Nanotube / Ti chlorine evolution anode material. This preparation method does not require a tedious brushing-sintering process, avoids the problem of easy cracking of electrodes prepared by traditional thermal decomposition methods, and provides a new method for designing and developing efficient chlorine evolution anodes. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The Cu-RuO of Example 1 of the present invention 2 / TiO 2 Scanning electron microscope (SEM) image of nanotube / Ti chlorine evolution anode material;
[0025] Figure 2 The Cu-RuO of Example 1 of the present invention 2 / TiO 2 Energy dispersive spectrometer (EDS) diagram of nanotube / Ti chlorine evolution anode material;
[0026] Figure 3 The Cu-RuO of Example 1 of the present invention 2 / TiO 2 X-ray photoelectron spectroscopy (XPS) of nanotube / Ti chlorine evolution anode material;
[0027] Figure 4 The Cu-RuO of Example 1 of the present invention 2 / TiO 2 XPS fine spectrum of Cu 2p of nanotube / Ti chlorine evolution anode material;
[0028] Figure 5 The RuO in Comparative Example 2 2 / TiO 2 Nanotube / Ti electrode material and Cu-RuO of Example 1 2 / TiO 2 The double layer capacitance (C dl )picture;
[0029] Figure 6 The RuO in Comparative Example 2 2 / TiO 2 Nanotube / Ti electrode material and Cu-RuO of Example 1 2 / TiO 2 Electrochemical impedance spectroscopy (EIS) of nanotube / Ti chlorine evolution anode material;
[0030] Figure 7 The RuO in Comparative Example 2 2 / TiO2 Nanotube / Ti electrode material and Cu-RuO of Example 1 2 / TiO 2 Polarization curves (LSV) of chlorine and oxygen evolution reactions of nanotube / Ti chlorine evolution anode materials;
[0031] Figure 8 This is the LSV diagram of the chlorine evolution reaction of the commercial DSA electrode in Example 1. DETAILED DESCRIPTION
[0032] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0033] The present invention Cu-RuO 2 / TiO 2 The preparation method of nanotube / Ti chlorine evolution anode material is to use a mixed solution of ammonium fluoride, water and ethylene glycol as an electrolyte, and to in-situ grow TiO on the surface of a Ti sheet by an anodic oxidation method. 2 Nanotubes, and then the Cu-RuO with high catalytic activity can be prepared by electrodeposition. 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution.
[0034] Follow the steps below to implement it:
[0035] Step 1, pretreatment of Ti sheet:
[0036] The Ti sheet was polished and cleaned with distilled water, then ultrasonically degreased and deoiled in a 0.01-1M sodium hydroxide solution, then placed in a 0.5-1.5M oxalic acid solution, and etched in a 70-90°C water bath for 1-3h to further remove the oxide layer. After cleaning, it was stored in ethanol for later use.
[0037] Step 2: In-situ growth of TiO on the surface of Ti sheet 2 Nanotubes:
[0038] A two-electrode system is used, a mixture of ammonium fluoride, water and ethylene glycol is used as the electrolyte, the Ti sheet pretreated in step 1 is used as the anode and the Pt mesh is used as the cathode, the Ti sheet is anodized at a constant voltage of 30 to 90 V, the anodization time is 10 to 60 min, and finally the temperature is raised to 350 to 550 ° C at a rate of 1 to 10 ° C / min in a muffle furnace, kept at this temperature for 1 to 4 hours, and cooled naturally to obtain TiO 2 Nanotube / Ti electrode.
[0039] In the electrolyte, the mass fraction of ammonium fluoride is 0.3-0.6 wt %, and the volume fraction of water is 2-5 vol %.
[0040] Step 3, Cu-RuO 2 / TiO2 Preparation of nanotube / Ti chlorine evolution anode material:
[0041] The TiO prepared in step 2 2 The nanotube / Ti electrode was used as cathode, the Pt mesh as anode, and a mixture of ruthenium chloride, copper nitrate trihydrate, aminosulfonic acid, potassium chloride, hydrochloric acid, and water as electrolyte at 5-20 mA / cm 2 The Cu-RuO was obtained by electro-depositing at a current density of 5 to 30 minutes, and finally heating to 350 to 550°C at a rate of 1 to 10°C / min in a muffle furnace, keeping the temperature for 1 to 4 hours, and cooling naturally. 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution.
[0042] In the electrolyte, the concentration of ruthenium chloride is 5 to 15 mM, the concentration of copper nitrate trihydrate is 0.05 to 5 mM, the concentration of aminosulfonic acid is 1 to 10 mM, the concentration of hydrochloric acid is 5 to 100 mM, and the concentration of potassium chloride is 0.05 to 1 M.
[0043] This step is the core step of the present invention. The TiO 2 In-situ preparation of RuO doped with Cu on the surface of nanotube / Ti sheet 2 Catalytic coating, regulating RuO by heterogeneous element Cu 2 At the same time, Cu doping reduces the adsorption energy of oxygen evolution reaction intermediates (HO*, O*, HOO*) on ruthenium active sites, delays the reaction kinetics of oxygen evolution reaction, and thus improves the selectivity and catalytic activity of chlorine evolution reaction.
[0044] The following is a specific example of the Cu-RuO 2 / TiO 2 The preparation method of nanotube / Ti chlorine evolution anode material is described.
[0045] Comparative Example 1
[0046] The comparative example is a commercial DSA electrode purchased directly without any treatment.
[0047] Comparative Example 2
[0048] Step 1, pretreatment of Ti sheet:
[0049] The Ti sheet was polished and cleaned with distilled water, then ultrasonically degreased in 0.1 M sodium hydroxide solution, and then placed in 1 M oxalic acid solution and etched in a water bath at 85 °C for 2 h to further remove the oxide layer. After cleaning, it was stored in ethanol for later use.
[0050] Step 2: In-situ growth of TiO on the surface of Ti sheet2 Nanotubes:
[0051] A two-electrode system was used, with a mixture of 0.5wt% ammonium fluoride, 3vol% water, and ethylene glycol as the electrolyte, the Ti sheet pretreated in step 1 as the anode, and the Pt mesh as the cathode. The Ti sheet was anodized at a constant voltage of 60V for 30min, and finally heated to 450℃ in a muffle furnace at a heating rate of 5℃ / min, and the holding time was 2h. After naturally cooling to room temperature, TiO 2 Nanotube / Ti electrode.
[0052] Step 3, RuO 2 / TiO 2 Preparation of nanotube / Ti electrode materials:
[0053] The TiO prepared in step 2 2 The nanotube / Ti electrode was used as the cathode and the Pt mesh as the anode. A mixture of 10 mM ruthenium chloride, 2 mM aminosulfonic acid, 0.1 M potassium chloride, 10 mM hydrochloric acid, and water was used as the electrolyte. The electrolyte was 10 mA / cm 2 Electrodeposition was performed at a current density of 15 min. Finally, the temperature was raised to 450 °C in a muffle furnace at a heating rate of 5 °C / min and the holding time was 2 h. After natural cooling, RuO 2 / TiO 2 Nanotube / Ti electrode material.
[0054] Example 1
[0055] Step 1, pretreatment of Ti sheet:
[0056] The Ti sheet was polished and cleaned with distilled water, then ultrasonically degreased in 0.1 M sodium hydroxide solution, and then placed in 1 M oxalic acid solution and etched in a water bath at 85 °C for 2 h to further remove the oxide layer. After cleaning, it was stored in ethanol for later use.
[0057] Step 2: In-situ growth of TiO on the surface of Ti sheet 2 Nanotubes:
[0058] A two-electrode system was used, with a mixture of 0.5wt% ammonium fluoride, 3vol% water, and ethylene glycol as the electrolyte, the Ti sheet pretreated in step 1 as the anode, and the Pt mesh as the cathode. The Ti sheet was anodized at a constant voltage of 60V for 30min, and finally heated to 450℃ in a muffle furnace at a heating rate of 5℃ / min, and the holding time was 2h. After naturally cooling to room temperature, TiO 2 Nanotube / Ti electrode.
[0059] Step 3, Cu-RuO 2 / TiO 2Preparation of nanotube / Ti chlorine evolution anode material:
[0060] The TiO prepared in step 2 2 The nanotube / Ti electrode was used as the cathode and the Pt mesh as the anode. A mixture of 10 mM ruthenium chloride, 0.15 mM copper nitrate trihydrate, 2 mM aminosulfonic acid, 0.1 M potassium chloride, 10 mM hydrochloric acid, and water was used as the electrolyte. The electrolyte was 10 mA / cm 2 The electrodeposition was carried out at a current density of 15 min. Finally, the temperature was raised to 450 °C in a muffle furnace at a heating rate of 5 °C / min and the holding time was 2 h. After natural cooling, Cu-RuO 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution.
[0061] Example 2
[0062] Step 1, pretreatment of Ti sheet:
[0063] The Ti sheet was polished and cleaned with distilled water, then ultrasonically degreased in 0.01 M sodium hydroxide solution, and then placed in 0.5 M oxalic acid solution and etched in a 70 °C water bath for 1 h to further remove the oxide layer. After cleaning, it was stored in ethanol for later use.
[0064] Step 2: In-situ growth of TiO on the surface of Ti sheet 2 Nanotubes:
[0065] A two-electrode system was used, with a mixture of 0.3wt% ammonium fluoride, 2vol% water, and ethylene glycol as the electrolyte, the Ti sheet pretreated in step 1 as the anode, and the Pt mesh as the cathode. The Ti sheet was anodized at a constant voltage of 30V for 10min, and finally heated to 350℃ in a muffle furnace at a heating rate of 5℃ / min, and the holding time was 1h. After naturally cooling to room temperature, TiO 2 Nanotube / Ti electrode.
[0066] Step 3, Cu-RuO 2 / TiO 2 Preparation of nanotube / Ti chlorine evolution anode material:
[0067] The TiO prepared in step 2 2 The nanotube / Ti electrode was used as the cathode and the Pt mesh as the anode. A mixture of 5 mM ruthenium chloride, 0.05 mM copper nitrate trihydrate, 1 mM aminosulfonic acid, 0.05 M potassium chloride, 5 mM hydrochloric acid, and water was used as the electrolyte. The electrolyte was 10 mA / cm 2 The electrodeposition was carried out at a current density of 5 min. Finally, the temperature was raised to 550 °C in a muffle furnace at a heating rate of 5 °C / min and the holding time was 4 h. After natural cooling, Cu-RuO 2 / TiO2 Nanotube / Ti anode material for chlorine evolution.
[0068] Example 3
[0069] Step 1, pretreatment of Ti sheet:
[0070] The Ti sheet was polished and cleaned with distilled water, then ultrasonically degreased and deoiled in a 0.5 M sodium hydroxide solution, then placed in a 1 M oxalic acid solution and etched in a 90 °C water bath for 3 h to further remove the oxide layer, and then stored in ethanol for later use.
[0071] Step 2: In-situ growth of TiO on the surface of Ti sheet 2 Nanotubes:
[0072] A two-electrode system was used, with a mixture of 0.6 wt% ammonium fluoride, 5 vol% water, and ethylene glycol as the electrolyte, the Ti sheet pretreated in step 1 as the anode, and the Pt mesh as the cathode. The Ti sheet was anodized at a constant voltage of 60 V for 60 min, and finally heated to 450 ° C in a muffle furnace at a heating rate of 10 ° C / min, and the holding time was 3 h. After cooling naturally to room temperature, TiO 2 Nanotube / Ti electrode.
[0073] Step 3, Cu-RuO 2 / TiO 2 Preparation of nanotube / Ti chlorine evolution anode material:
[0074] The TiO prepared in step 2 2 The nanotube / Ti electrode was used as the cathode, the Pt mesh was used as the anode, and a mixture of 15 mM ruthenium chloride, 5 mM copper nitrate trihydrate, 10 mM aminosulfonic acid, 1 M potassium chloride, 100 mM hydrochloric acid, and water was used as the electrolyte at 20 mA / cm 2 The electrodeposition was carried out at a current density of 30 min. Finally, the temperature was raised to 550 °C in a muffle furnace at a heating rate of 10 °C / min and the holding time was 1 h. After natural cooling, Cu-RuO 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution.
[0075] Example 4
[0076] Step 1, pretreatment of Ti sheet:
[0077] The Ti sheet was polished and cleaned with distilled water, then ultrasonically degreased in 0.1 M sodium hydroxide solution, and then placed in 1.5 M oxalic acid solution and etched in a 90 °C water bath for 3 h to further remove the oxide layer. After cleaning, it was stored in ethanol for later use.
[0078] Step 2: In-situ growth of TiO on the surface of Ti sheet 2Nanotubes:
[0079] A two-electrode system was used, with a mixture of 0.5wt% ammonium fluoride, 4vol% water, and ethylene glycol as the electrolyte, the Ti sheet pretreated in step 1 as the anode, and the Pt mesh as the cathode. The Ti sheet was anodized at a constant voltage of 40V for 40min, and finally heated to 550℃ in a muffle furnace at a heating rate of 1℃ / min, and the holding time was 3h. After naturally cooling to room temperature, TiO 2 Nanotube / Ti electrode.
[0080] Step 3, Cu-RuO 2 / TiO 2 Preparation of nanotube / Ti chlorine evolution anode material:
[0081] The TiO prepared in step 2 2 The nanotube / Ti electrode was used as the cathode, the Pt mesh was used as the anode, and a mixture of 5 mM ruthenium chloride, 0.05 mM copper nitrate trihydrate, 1 mM aminosulfonic acid, 1 M potassium chloride, 50 mM hydrochloric acid, and water was used as the electrolyte at 5 mA / cm 2 The electrodeposition was carried out at a current density of 30 min. Finally, the temperature was raised to 550 °C in a muffle furnace at a heating rate of 1 °C / min and the holding time was 1 h. After natural cooling, Cu-RuO 2 / TiO 2 Nanotube / Ti anode material for chlorine evolution.
[0082] The structural characterization and electrocatalytic chlorine evolution performance test of the above comparative example and embodiment chlorine evolution anode materials were carried out, and the results are as follows:
[0083] Cu-RuO of Example 1 of the present invention 2 / TiO 2 SEM photos of nanotube / Ti chlorine evolution anode materials are shown in Figure 1 As shown in the figure, it can be seen that when Cu-RuO is loaded 2 After catalytic coating, TiO 2 The mouth and wall of the nanotube are loaded with a large amount of nanoparticles. 2 / TiO 2 EDS of nanotube / Ti chlorine evolution anode material ( Figure 2 ) shows that the constituent elements of this electrode are Ru, Cu, Ti, and O. Figure 3 The Cu-RuO of Example 1 2 / TiO 2 The XPS spectrum of the nanotube / Ti chlorine evolution anode material shows the signal peaks of four elements: Ru, Cu, Ti, and O. 2 / TiO 2High-resolution XPS spectrum of Cu 2p of nanotube / Ti chlorine evolution anode material ( Figure 4 ) we can see that Cu appeared at 932.6eV and 952.3eV respectively. 2+ Cu 2p 3 / 2 and Cu 2p 1 / 2 The above results show that Cu-RuO 2 / TiO 2 Nanotube / Ti chlorine evolution anode material was successfully prepared.
[0084] The specific method of testing the electrochemical chlorine evolution performance of the comparative example and the embodiment chlorine evolution anode materials prepared by the present invention is as follows:
[0085] The electrochemical test of the three-electrode system was carried out on a Shanghai Chenhua electrochemical workstation, wherein the reference electrode was a saturated calomel electrode, the auxiliary electrode was a Pt mesh electrode, and the working electrode was the chlorine evolution anode material prepared in the comparative example and the embodiment.
[0086] Figure 5 The RuO in Comparative Example 2 2 / TiO 2 Nanotube / Ti electrode material and Cu-RuO of Example 1 2 / TiO 2 Nanotube / Ti anode materials for chlorine evolution dl From the figure, we can see that the active area of the electrode after doping with Cu element is larger and has more catalytic active sites. Figure 6 The RuO in Comparative Example 2 2 / TiO 2 Nanotube / Ti electrode material and Cu-RuO of Example 1 2 / TiO 2 From the EIS graph of nanotube / Ti chlorine evolution anode material, it can be seen that the addition of Cu element reduces the charge transfer resistance and improves the electron transmission efficiency. Figure 7 The RuO in Comparative Example 2 2 / TiO 2 Nanotube / Ti electrode material and Cu-RuO of Example 1 2 / TiO 2 LSV diagram of oxygen evolution and chlorine evolution reaction of nanotube / Ti chlorine evolution anode material. It can be seen from the figure that at 10mA / cm 2 At a current density of , the chlorine evolution reaction (CER) potential of Comparative Example 2 is 1.108 V, and the oxygen evolution reaction (OER) potential is 1.275 V; the chlorine evolution reaction potential of Example 1 is 1.081 V, and the oxygen evolution reaction potential is 1.324 V. The chlorine-oxygen potential differences of Comparative Example 2 and Example 1 are 167 mV and 243 mV, respectively, indicating that the chlorine-oxygen potential difference of the electrode is significantly increased after doping with the Cu element. Figure 8This is the LSV diagram of the chlorine evolution reaction of the commercial DSA electrode of Example 1. It can be seen from the figure that at 10mA / cm 2 At a current density of , the chlorine evolution reaction potential of Comparative Example 1 is 1.130V. Therefore, the chlorine evolution reaction potential of Example 1 of the present invention is 49mV lower than that of Comparative Example 2, indicating that its electrocatalytic chlorine evolution performance is better than that of commercial DSA electrodes on the market. In summary, after doping with the Cu element, the selectivity and catalytic activity of the chlorine evolution reaction of the chlorine evolution anode material are significantly improved.
[0087] RuO 2 It is a classic catalyst in the field of electrocatalytic chlorine evolution. It can significantly reduce the reaction energy barrier and increase the rate of chlorine generation. However, since the chlorine evolution reaction and the oxygen evolution reaction involve the same reaction intermediate, the Ru-based electrode has limited electrochemical oxidation selectivity for chloride ions in aqueous solution. In view of this, the present invention selects the Cu element to RuO 2 Doping can reduce the adsorption energy of oxygen evolution reaction intermediates (HO*, O*, HOO*) on Ru active sites and slow down the reaction kinetics of oxygen evolution reaction. 2 Its electronic structure can be regulated to change the electrode potential of the chlorine evolution reaction, thereby improving the selectivity and catalytic activity of the chlorine evolution reaction.
Claims
1. A method for preparing a Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material, characterized in that: Using a mixture of ammonium fluoride, water and ethylene glycol as the electrolyte, TiO2 nanotubes are in situ grown on the surface of the Ti sheet by an anodic oxidation method, and then a Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material with high catalytic activity can be prepared by an electrodeposition method.
2. The method for preparing the Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material according to claim 1, characterized in that: Follow the steps below to implement it: Step 1, pretreatment of Ti sheet: The Ti sheet was polished and cleaned with distilled water, then ultrasonically degreased in a 0.01-1M sodium hydroxide solution, and then placed in a 0.5-1.5M oxalic acid solution and etched in a water bath for several hours to further remove the oxide layer. After cleaning, it was stored in ethanol for later use. Step 2: In-situ growth of TiO2 nanotubes on the surface of Ti sheet: A two-electrode system is used, a mixed solution of ammonium fluoride, water and ethylene glycol is used as an electrolyte, the Ti sheet pretreated in step 1 is used as an anode and the Pt mesh is used as a cathode, the Ti sheet is subjected to an anodic oxidation treatment, and finally the temperature is raised to 350-550°C at a rate of 1-10°C / min in a muffle furnace, kept at this temperature for 1-4 hours, and cooled naturally, thereby obtaining a TiO2 nanotube / Ti electrode; Step 3, preparation of Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material: The TiO2 nanotube / Ti electrode prepared in step 2 is used as the cathode and the Pt mesh is used as the anode. A mixed solution of ruthenium chloride, copper nitrate trihydrate, aminosulfonic acid, potassium chloride, hydrochloric acid and water is used as the electrolyte for electrodeposition treatment. Finally, the temperature is raised to 350-550°C at a rate of 1-10°C / min in a muffle furnace, kept at this temperature for 1-4h, and cooled naturally to obtain Cu-RuO 2 / TiO2 nanotube / Ti chlorine evolution anode material.
3. The method for preparing the Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material according to claim 2, characterized in that: In the step 1, the water bath etching temperature is 70 to 90° C., and the etching time is 1 to 3 hours.
4. The method for preparing the Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material according to claim 2, characterized in that: In the step 2, the voltage of the anodization is 30 to 90 V, and the time is 10 to 60 minutes.
5. The method for preparing the Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material according to claim 2, characterized in that: In step 3, the current density of the electrodeposition is 5 to 20 mA / cm 2 , time is 5 to 30 minutes.
6. The method for preparing the Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material according to claim 2, characterized in that: In step 3, in the electrolyte, the concentration of ruthenium chloride is 5-15 mM, the concentration of copper nitrate trihydrate is 0.05-5 mM, the concentration of aminosulfonic acid is 1-10 mM, the concentration of hydrochloric acid is 5-100 mM, and the concentration of potassium chloride is 0.05-1 M. 7.Cu-RuO2 / TiO2 nanotube / Ti chlorine evolution anode material, characterized in that: The method is prepared by any one of claims 1 to 6.
Citation Information
Cited By