AEM electrolyzed water anode material based on MOF derivation as well as laser preparation method and application of AEM electrolyzed water anode material

By combining the MOF material ZIF-67 with Fe-Phen, the AEM electrolytic anode material is prepared by using direct laser scribe technology, which solves the scarcity and high cost of precious metal catalysts, and achieves efficient and stable electrolytic hydrogen production, which simplifies the Process flow and reduce costs.

CN118932401AActive Publication Date: 2024-11-12ZHEJIANG UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411113985.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The precious metal catalysts used in existing AEM electrolytic devices are scarce, costly and have low catalytic performance. The preparation process of the powder catalyst loading to the electrode is complicated, and the introduction of binders reduces the conductivity of the catalyst and the support.

Method used

The MOF material ZIF-67 is mixed with Fe-Phen, and anode electrode material with high activity and stability is prepared through direct laser scribe technology. By optimizing process parameters and raw material types, the defects of the traditional method are solved.

Benefits of technology

The prepared AEM electrolytic water anode material based on MOF derived has high efficiency catalytic activity and stability, and is simple in process and low in cost. It is suitable for mass production, which significantly improves the hydrogen production efficiency of electrolytic water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004993111760000011
    Figure HDA0004993111760000011
  • Figure HDA0004993111760000012
    Figure HDA0004993111760000012
  • Figure HDA0004993111760000021
    Figure HDA0004993111760000021
Patent Text Reader

Abstract

The invention discloses an AEM electrolyzed water anode material based on MOF derivation and a laser preparation method and application thereof.The method includes the steps that a ZIF-67 (Co) material is formed through a mechanical stirring method, Fe-Phen is added, then the ZIF-67 (Co) material is quantitatively loaded on carbon paper, a network-shaped alloy material is formed through a direct laser scribing technology, more active sites are exposed due to the network-shaped structure, and therefore the anode material can be applied to water electrolysis; the formed Co and Fe alloy has a promoting effect on OER performance, and the problems that an original MOF material is poor in conductivity and low in electrocatalytic activity are solved; meanwhile, the electrocatalyst and the electrode are formed in a one-time composite mode, and complex processes and adverse factors caused by loading of a powder catalyst material are avoided; the overpotential of the prepared material reaches up to 250 mV in an electro-catalysis test, and the material has excellent electro-catalysis activity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of water electrolysis devices and water electrolysis processes, and specifically relates to a MOF-derived oxygen evolution catalyst and a preparation method and application thereof by laser rapid heating. Background Art

[0002] We urgently need to develop renewable energy to reduce our dependence on fossil fuels. Hydrogen has always been recognized as the most promising green energy carrier. It has the characteristics of high energy density, easy transportation, clean and pollution-free energy release process, and abundant reserves. It is an important raw material for fertilizer production, petroleum refining and hydrogenation in industry. Producing "green hydrogen" through electrocatalytic water splitting is a sustainable method with high efficiency and broad application prospects.

[0003] The main water electrolysis processes include alkaline water electrolysis (AWE), proton exchange membrane (PEM) and anion exchange membrane (AEM). AEM has attracted widespread attention due to its high hydrogen production efficiency and its lower cost-effectiveness than PEM (transition metal catalysts can be used instead of platinum group metal catalysts, the membrane used in AEM electrolysis is cheaper than Nafion membrane, and stainless steel can be used instead of Ti as a porous transport layer and bipolar plate in AEM electrolysis). In AEM water electrolysis devices, electrocatalysts greatly affect the efficiency of hydrogen production by water electrolysis, so the design and preparation of electrocatalysts with high activity and stability are of great significance to promote the development of water electrolysis. Metal organic framework (MOF) materials can be used as good precursors for the synthesis of efficient catalysts because of their advantages such as high specific surface area, adjustable pore size and clear metal nodes. Composite materials based on three-dimensional transition metals such as iron, cobalt, and nickel can generally be used as OER catalysts to replace commercial precious metals.

[0004] Direct laser scribing is an advanced printing technology that can convert non-conductive materials into active electrode materials according to a set pattern through laser. Compared with traditional methods, this preparation method is faster, cheaper, and can print fine patterns with high precision. Here, we propose to use MOF materials as precursors, introduce metallic iron-1,10-phenanthroline complexes (Fe-Phen), and use direct laser scribing technology to quickly heat and prepare electrocatalysts with high activity and stability for water electrolysis. Summary of the invention

[0005] The present invention provides an anode material for AEM water electrolysis based on MOF, and a preparation method and application thereof. The present invention mixes ZIF-67 with Fe-Phen and prepares an anode terminal electrode with high activity and stability for AEM water electrolysis by a direct laser scribing method, selects and optimizes the process parameters and raw material types in the preparation process, solves the problems of scarcity, high price and low catalytic efficiency of traditional precious metal catalysts, as well as the complex preparation process of powder catalyst loading on the electrode, and the introduction of a binder to reduce the conductivity of the catalyst and the carrier.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing an AEM water electrolysis anode material based on MOF derivatives comprises the following steps:

[0008] (1) Preparation of ZIF-67: Cobalt nitrate hexahydrate solution and 2-methylimidazole solution were mixed, allowed to stand at room temperature, and then centrifuged and washed to obtain ZIF-67;

[0009] The mass ratio of cobalt nitrate hexahydrate to 2-methylimidazole is 0.58-2.89:0.66-3.29, preferably 1.82:2.06;

[0010] The preparation method of the cobalt nitrate hexahydrate solution is as follows: adding the cobalt nitrate hexahydrate to a mixed solvent of methanol and ethanol in a volume ratio of 1:1, and stirring evenly at room temperature to obtain the cobalt nitrate hexahydrate solution; the concentration of the cobalt nitrate hexahydrate solution is 0.02-0.1M, preferably 0.063M;

[0011] The preparation method of 2-methylimidazole solution is as follows: adding 2-methylimidazole solution to a mixed solvent of methanol and ethanol in a volume ratio of 1:1, stirring evenly at room temperature to obtain; the concentration of 2-methylimidazole solution is 0.08-0.4M, preferably 0.25M;

[0012] Specifically, the operation method of step (1) is as follows: inject the cobalt nitrate hexahydrate solution and the 2-methylimidazole solution into the reaction container at the same time, vigorously stir at 500-800 rpm (preferably 700 rpm) for 30 seconds, stand at room temperature for 18-24 hours (preferably 22 hours), centrifuge the suspension and wash it with ethanol three times, and the resulting precipitate is ZIF-67;

[0013] (2) Preparation of L-Fe-Co / C-CP: The ZIF-67 obtained in step (1), ferrous inorganic salt, and 1,10-phenanthroline monohydrate are uniformly stirred in a mixed solvent of ethanol and water, the obtained suspension is centrifuged, ethanol is added to the precipitate for ultrasonic dispersion, the obtained dispersion is evenly dropped on the surface of carbon paper, and the obtained material after ethanol is evaporated is recorded as Fe-ZIF-67-CP; Fe-ZIF-67-CP is carbonized by direct laser scribing to obtain the MOF-derived AEM water electrolysis anode material, which is recorded as L-Fe-Co / C-CP;

[0014] Preferably, the ferrous inorganic salt is ferrous sulfate heptahydrate;

[0015] The mass ratio of ZIF-67, 1,10-phenanthroline monohydrate, and ferrous inorganic salt is 1:0.8-1.2:0.6-1, preferably 1:1:0.82;

[0016] In the mixed solvent of ethanol and water, the volume ratio of ethanol to water is 1-3:1, preferably 2:1;

[0017] Specifically, ZIF-67, ferrous inorganic salt, and 1,10-phenanthroline monohydrate are stirred in a mixed solvent of ethanol and water at room temperature for 2-4 hours (preferably 3 hours) at a stirring speed of 200-400 rpm (preferably 300 rpm);

[0018] The amount of dispersion added to the carbon paper surface is 3-8 mg / cm -2 , preferably 6mg / cm -2 ;

[0019] The parameters of direct laser scribing are set as follows: laser power 1.7-10.2 W (preferably 5.59 W), scribing spacing 100-180 μm (preferably 150 μm).

[0020] The invention relates to an AEM water electrolysis anode material based on MOF derived and prepared by the preparation method.

[0021] The MOF-derived AEM water electrolysis anode material of the present invention can be used in the reaction of water electrolysis. The MOF-derived AEM water electrolysis anode material can be assembled as an anode in an AEM water electrolysis device to perform a water electrolysis test.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention provides an AEM water electrolysis anode material based on MOF. First, ZIF-67 is synthesized, and the morphology of ZIF-67 is found to be dodecahedron by SEM. After the metal Fe element is introduced, it is loaded on carbon paper and carbonized by direct laser scribing technology. Characterization by SEM and HRTEM shows that the morphology of ZIF-67 has undergone a drastic change, from the original dodecahedron to a network-like structure, exposing more active sites and having efficient catalytic activity.

[0024] The electrode material prepared by mixing MOF material ZIF-67 with Fe-Phen and carbonizing it by direct laser scribing technology has good catalytic activity and stability. The method of the invention is simple and easy to operate, low in cost, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 : Scanning electron microscopy images of ZIF-67 in Examples 1-14.

[0026] Figure 2 : Scanning electron microscope image of Fe-ZIF-67 in Example 2.

[0027] Figure 3 : Scanning electron microscope image of sample 1 in Example 1.

[0028] Figure 4 : Scanning electron microscope image of sample 2 in Example 2.

[0029] Figure 5 : Scanning electron microscope image of sample 3 in Example 3.

[0030] Figure 6 : Scanning electron microscope image of sample 4 in Example 4.

[0031] Figure 7 : Electrocatalytic performance diagram of sample 1, sample 2, sample 3, sample 4, and sample 5.

[0032] Figure 8 : Electrochemical impedance diagrams of sample 1, sample 2, sample 3, sample 4, and sample 5.

[0033] Fig. 9 :AEM water electrolysis device assembled with sample 1 as anode at 10 mA cm -2 The voltage stability diagram of the electrolyzer below. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0035] In the following examples, the manufacturer of the carbon paper is Suzhou Shengernuo Technology Co., Ltd., the brand is Toray, and the model is TGP-H-060, a relatively hydrophilic carbon paper.

[0036] Embodiment 1:

[0037] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature for 22 h (the same standing time below). ZIF-67 was obtained after centrifugation and washing.

[0038] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 475.6 mg 1,10-phenanthroline monohydrate were stirred magnetically for 3 h in a mixed solution of ethanol and water (40 mL ethanol and 20 mL water, the same in other embodiments) with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP (M is Fe, the same below). Sample 1 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as a laser power of 5.59 W and a scribing spacing of 150 μm.

[0039] Embodiment 2:

[0040] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0041] 200 mg ZIF-67, 13.9 mg ferrous sulfate heptahydrate, and 29.73 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. Sample 2 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as a laser power of 5.59 W and a scribing spacing of 150 μm.

[0042] Embodiment 3:

[0043] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0044] 200 mg ZIF-67, 55.6 mg ferrous sulfate heptahydrate, and 118.9 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. Sample 3 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as a laser power of 5.59 W and a scribing spacing of 150 μm.

[0045] Embodiment 4:

[0046] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0047] 200 mg ZIF-67, 333.6 mg ferrous sulfate heptahydrate, and 713.4 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. Sample 4 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as a laser power of 5.59 W and a scribing spacing of 150 μm.

[0048] Embodiment 5:

[0049] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0050] After ultrasonic homogenization, 6 mg of ZIF-67 was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as ZIF-67-CP. Sample 5 was obtained by carbonizing ZIF-67-CP using direct laser scribing technology with laser parameters such as a laser power of 5.59 W and a scribing spacing of 150 μm.

[0051] Embodiment 6:

[0052] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0053] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 158.53 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. Sample 6 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as a laser power of 5.59 W and a scribing spacing of 150 μm.

[0054] Embodiment 7:

[0055] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0056] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 475.6 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. Sample 7 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as 3.4 W laser power and 150 μm scribing spacing.

[0057] Embodiment 8:

[0058] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0059] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 475.6 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. Sample 8 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as a laser power of 5.59 W and a scribing spacing of 150 μm.

[0060] Embodiment 9:

[0061] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0062] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 475.6 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. Sample 9 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as 8.5 W laser power and 150 μm scribing spacing.

[0063] Embodiment 10:

[0064] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0065] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 475.6 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. The M-ZIF-67-CP was carbonized by direct laser scribing technology with laser parameters such as 11.05 W laser power and 150 μm scribing spacing to obtain sample 10.

[0066] Embodiment 11:

[0067] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0068] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 475.6 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. The M-ZIF-67-CP was carbonized by direct laser scribing technology with laser parameters such as 5.59 W laser power and 120 μm scribing spacing to obtain sample 11.

[0069] Embodiment 12:

[0070] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0071] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 475.6 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2The carbon paper was marked as M-ZIF-67-CP. The M-ZIF-67-CP was carbonized by direct laser scribing technology with laser parameters such as 5.59 W laser power and 140 μm scribing spacing to obtain sample 12.

[0072] Embodiment 13:

[0073] 1.82 g of cobalt nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0074] 200 mg ZIF-67, 222.4 mg ferrous sulfate heptahydrate, and 475.6 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. Sample 13 was obtained by carbonizing M-ZIF-67-CP using direct laser scribing technology with laser parameters such as 5.59 W laser power and 160 μm scribing spacing.

[0075] Embodiment 14:

[0076] 1.82 g of zinc nitrate hexahydrate was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. 2.06 g of 2-methylimidazole was added to 100 mL of a mixed solution of methanol and ethanol in a volume ratio of 1:1 and mixed evenly. The above two solutions were simultaneously injected into a glass bottle and stirred vigorously and then allowed to stand at room temperature. ZIF-67 was obtained after centrifugation and washing.

[0077] 200 mg ZIF-67, 164 mg ferrous sulfate heptahydrate, and 200 mg 1,10-phenanthroline monohydrate were magnetically stirred for 3 h in a mixed solution of ethanol and water with a volume ratio of 2:1. The obtained suspension was centrifuged and then added with ethanol solution. After ultrasonic homogenization, 6 mg was quantitatively dropped on a 1×1 cm -2 The carbon paper was marked as M-ZIF-67-CP. The M-ZIF-67-CP was carbonized by direct laser scribing technology with laser parameters such as 5.59 W laser power and 180 μm scribing spacing to obtain sample 14.

[0078] Figure 1This is a scanning electron microscope image of ZIF-67 in Example 1-14. It is observed that the obtained ZIF-67 has a dodecahedral morphology and a uniform particle size.

[0079] Figure 2 This is a scanning electron microscope image of Fe-ZIF-67 in Example 2. It is observed that after the Fe element is doped, the surface of the sample is slightly rough and evenly distributed.

[0080] Figure 3 This is a scanning electron microscope image of sample 1 in Example 1. It is observed that the morphology of the sample undergoes a huge change after laser treatment, presenting a network structure that can expose more active sites.

[0081] Figure 4 This is a scanning electron microscope image of sample 2 in Example 2. It is observed that the morphology of the sample after laser treatment also presents a network structure.

[0082] Figure 5 This is a scanning electron microscope image of sample 3 in Example 3. It is observed that the morphology of the sample after laser treatment also presents a network structure.

[0083] Figure 6 This is a scanning electron microscope image of sample 4 in Example 4. It is observed that the morphology of the sample after laser treatment also presents a network structure.

[0084] Figure 7 The electrocatalytic performance diagram of sample 1, sample 2, sample 3, sample 4, and sample 5 shows that the different Fe doping contents have a certain influence on the final performance. Sample 1 formed after Fe doping and laser treatment has more active sites, 10 mA cm -2 The overpotential is 250mV.

[0085] Figure 8 The electrochemical impedance diagrams of sample 1, sample 2, sample 3, sample 4 and sample 5 show that the impedance of the sample is reduced after the addition of Fe, and with the addition of Fe element, it shows a trend of first decreasing and then increasing. The impedance value of sample 1 is the smallest.

[0086] Fig. 9 The voltage of the electrolyzer of the AEM water electrolysis device assembled with sample 1 as the anode varies with time. Sample 1 is used as the anode and commercial Pt / C is used as the cathode. The stability is tested by chronopotentiometry. It is found that at 10 mA cm -2 At a current density of , the battery voltage is maintained at 1.57V. After testing for nearly 80h, the potential change is about 20mV. The stability is good.

[0087] The preferred embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. All experiments and technical solutions that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing an AEM water electrolysis anode material based on MOF, characterized in that: The steps include: (1) Preparation of ZIF-67: Cobalt nitrate hexahydrate solution and 2-methylimidazole solution were mixed, allowed to stand at room temperature, and then centrifuged and washed to obtain ZIF-67; (2) Preparation of L-Fe-Co / C-CP: The ZIF-67, ferrous inorganic salt and 1,10-phenanthroline monohydrate obtained in step (1) are uniformly stirred in a mixed solvent of ethanol and water, the obtained suspension is centrifuged, ethanol is added to the precipitate and ultrasonically dispersed uniformly, the obtained dispersion is evenly dropped on the surface of carbon paper, and the material obtained after evaporation of the ethanol is recorded as Fe-ZIF-67-CP; Fe-ZIF-67-CP is carbonized by direct laser scribing to obtain the MOF-derived AEM water electrolysis anode material, which is recorded as L-Fe-Co / C-CP.

2. The method for preparing an AEM water electrolysis anode material based on MOF as claimed in claim 1, characterized in that: In step (1), the mass ratio of cobalt nitrate hexahydrate to 2-methylimidazole is 0.58-2.89:0.66-3.

29.

3. The method for preparing an AEM water electrolysis anode material based on MOF as claimed in claim 1, characterized in that: In step (1), the preparation method of the cobalt nitrate hexahydrate solution is: adding cobalt nitrate hexahydrate to a mixed solvent of methanol and ethanol in a volume ratio of 1:1, and stirring evenly at room temperature to obtain the cobalt nitrate hexahydrate solution; the concentration of the cobalt nitrate hexahydrate solution is 0.02-0.1M; The preparation method of the 2-methylimidazole solution is as follows: adding the 2-methylimidazole solution to a mixed solvent of methanol and ethanol in a volume ratio of 1:1, stirring evenly at room temperature, and obtaining the solution; the concentration of the 2-methylimidazole solution is 0.08-0.4M.

4. The method for preparing an AEM water electrolysis anode material based on MOF as claimed in claim 1, characterized in that: In step (1), the operation method is as follows: inject the cobalt nitrate hexahydrate solution and the 2-methylimidazole solution into the reaction container at the same time, vigorously stir at 500-800 rpm for 30 seconds, stand at room temperature for 18-24 hours, centrifuge the suspension and wash it with ethanol three times, and the resulting precipitate is ZIF-67.

5. The method for preparing an AEM water electrolysis anode material based on MOF as claimed in claim 1, characterized in that: In step (2), the ferrous inorganic salt is ferrous sulfate heptahydrate.

6. The method for preparing an AEM water electrolysis anode material based on MOF as claimed in claim 1, characterized in that: In step (2), the mass ratio of ZIF-67, 1,10-phenanthroline monohydrate and ferrous inorganic salt is 1:0.8-1.2:0.6-1.

7. The method for preparing an AEM water electrolysis anode material based on MOF as claimed in claim 1, characterized in that: In step (2), ZIF-67, ferrous inorganic salt, and 1,10-phenanthroline monohydrate are stirred in a mixed solvent of ethanol and water at room temperature for 2-4 hours at a stirring speed of 200-400 rpm.

8. The method for preparing an AEM water electrolysis anode material based on MOF as claimed in claim 1, characterized in that: In step (2), the parameters of direct laser scribing are set as follows: laser power 1.7-10.2 W, scribing spacing 100-180 μm.

9. A MOF-derived AEM water electrolysis anode material prepared according to the preparation method of any one of claims 1 to 8.

10. Use of the MOF-derived AEM water electrolysis anode material as claimed in claim 9 in a water electrolysis reaction.

Citation Information

Patent Citations

  • Three-dimensional multifunctional graphene film and preparation method thereof

    CN115739013A

  • Method for synchronously realizing rapid carbonization of MOF (Metal Organic Framework) array and rapid self-generation of CNTs (Carbon Nanotubes) on surface

    CN116947023A