Cathode material for aluminum electrolysis and preparation method thereof
By preparing composite coatings of TiB2, fluorinated graphene, CNT and epoxy resin on the cathode material, and using silane reagent and dopamine as transition layers, the problem of poor bonding strength between the TiB2 coating and the matrix material is solved, and the problem of improvement of the Wetting, impact resistance and corrosion resistance of the cathode.
Patent Information
- Application Number
- CN202411050996.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The bonding strength between the existing TiB2 coating and the matrix material is poor, resulting in the cathode being easily shedded and insufficient impact resistance and corrosion resistance.
The composite coating is prepared by TiB2, fluorinated graphene, CNT, epoxy resin and diluent, and the combination strength of the substrate and the coating is enhanced by using silane reagent and dopamine as the transition layer, and the mechanical properties and resistance of the coating are enhanced by combining heat treatment. Corrosive.
It improves the wettability, resistance to high-temperature melt corrosion and mechanical properties of the cathode material, enhances the bonding strength between the coating and the substrate, and improves the impact resistance and corrosion resistance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum electrolysis, and in particular to a cathode material for aluminum electrolysis and a preparation method thereof. Background Art
[0003] Current research shows that TiB2 has excellent high temperature resistance, corrosion resistance, and good wettability to aluminum liquid. Therefore, TiB2 is used as a raw material to prepare TiB2 ceramic cathode material or to prepare TiB2 coating to wet the cathode material. Although TiB2 is the preferred ceramic cathode material, it has poor sintering density due to its high melting point and low diffusion coefficient. It also needs to be obtained by hot pressing sintering or cold pressing sintering with the addition of sintering aids. However, hot pressing sintering is expensive, and the application field is limited due to abnormal grain growth caused by chemical bond differences during the sintering process. Therefore, TiB2 coating is widely used due to its good performance and convenient operation. Although TiB2 coating can greatly improve the wettability of the cathode to aluminum liquid, the coating material has poor bonding strength with the substrate, which makes it easy to fall off, further resulting in poor impact resistance and corrosion resistance of the cathode. Summary of the invention
[0004] Technical problems solved by the present invention:
[0005] It is used to solve the problem of poor bonding strength between the TiB2 coating and the base material in the current cathode material.
[0006] The technical solution adopted by the present invention is:
[0007] In view of the above technical problems, the object of the present invention is to provide a cathode material for aluminum electrolysis and a preparation method thereof.
[0008] Based on this, the specific implementation plan is:
[0009] A method for preparing a cathode material for aluminum electrolysis comprises the following steps:
[0010] (1) Pretreatment of the base material
[0011] After cleaning, the base material is immersed in an acidic solution, which is a mixture of concentrated sulfuric acid (95-98%) and hydrogen peroxide (30%), with a volume ratio of 7:3. After 30 minutes of treatment, it is taken out and dried with N2. After drying, it is ready for use. The base material can be a carbon block or alloy block commonly used in the cathode of the electrolytic cell.
[0012] (2) Fabrication of composite coating on the surface of substrate material
[0013] The pretreated substrate material (1) is placed in a first treatment liquid, treated for 30 minutes, and then washed with deionized water to obtain a treated body 1 for use; the first treatment liquid is a 5 mM silane reagent solution, specifically (3-aminopropyl) triethoxysilane dissolved in a solvent, and the solvent is V (acetone): V (water) = 5:1.
[0014] Immerse treated body 1 in the second treatment liquid, treat for 6 to 10 hours, take out, wash with deionized water, and dry with N2 to obtain treated body 2 for use; the second treatment liquid is obtained by dissolving dopamine in Tris·HCl aqueous solution (10mM, pH8.5), and the ratio of dopamine to Tris·HCl aqueous solution is 0.01g:2.5~10mL.
[0015] The third treatment liquid is coated on the surface of the treatment body 2 to form a coating layer. After the coating layer is solidified, it is carbonized and cooled to room temperature to obtain a cathode material for aluminum electrolysis.
[0016] The raw material components of the third treatment liquid include TiB2, fluorinated graphene, CNT, epoxy resin, and diluent, and the ratio of the components is 30-50:15-40:1-5:20-35:1-5. The diluent includes at least one of ethylene glycol and diethylenetriamine. The average particle size of TiB2 is D 50 The diameter of the CNT is 10-40 nm and the length is 10-30 μm. The CNT can be selected from CNT materials or copper-plated CNTs. The copper-plated CNTs can be prepared by conventional methods. The fluorinated graphene has a fluorine-carbon ratio of 1. The above raw materials are weighed in proportion and evenly mixed to obtain a third treatment solution.
[0017] When coating the surface of the treated body 2, care should be taken to ensure that the coating surface is smooth and the thickness is uniform.
[0018] The coating layer is first allowed to stand at room temperature for 18 to 30 hours, and then placed in a heating furnace for heat treatment, first heating to 100°C at a rate of 20°C / h and holding for 1 to 3 hours, then heating to 150°C at a rate of 20°C / h and holding for 1 to 3 hours; then, heating to 200°C at a rate of 25°C, heating to 400°C at a rate of 20°C / h, heating to 600°C at a rate of 20°C / h, and heating to 900°C at a rate of 20°C / h, and keeping warm for 8 to 10 hours.
[0019] The technical mechanism and beneficial effects adopted by the present invention are as follows:
[0020] (1) The cathode material for aluminum electrolysis provided by the present invention, TiB2, fluorinated graphene, CNT, epoxy resin, and diluent are used as raw materials to prepare the coating liquid, which is applied to the surface of the substrate, not only so that it can have the advantage of good wettability with aluminum liquid, but also can well resist high-temperature melt erosion. At the same time, fluorinated graphene not only has excellent mechanical properties, but also has corrosion resistance. Adding CNT, CNT can improve the mechanical properties of the coating together with fluorinated graphene, and copper plating of CNT can prevent CNT from reacting with Al to form Al4C3, thereby preventing the coating from falling off.
[0021] (2) The cathode material for aluminum electrolysis provided by the present invention is prepared by treating the base material and using a silane reagent and dopamine as a transition layer to construct a composite coating, thereby enhancing the bonding strength between the base material and the coating, thereby achieving the purpose of improving impact resistance.
[0022] <Example>
[0023] Example 1
[0024] This embodiment provides a method for preparing a cathode material for aluminum electrolysis, comprising the following steps:
[0025] (1) Pretreatment of the base material
[0026] The base material is a carbon block. After cleaning, the base material is immersed in an acid solution, which is a mixture of concentrated sulfuric acid (95-98%) and hydrogen peroxide (30%), with a volume ratio of concentrated sulfuric acid to hydrogen peroxide of 7:3. After treatment for 30 minutes, it is taken out and dried with N2. After drying, it is ready for use.
[0027] (2) Fabrication of composite coating on the surface of substrate material
[0028] The pre-treated substrate material of (1) is placed in a first treatment liquid, which is a 5 mM silane reagent solution, specifically (3-aminopropyl) triethoxysilane dissolved in a solvent, wherein the solvent is V (acetone): V (water) = 5:1. After treatment for 30 minutes, it is washed with deionized water to obtain a treated body 1 for standby use.
[0029] The treated body 1 is immersed in the second treatment liquid, which is obtained by dissolving dopamine in a Tris·HCl aqueous solution (10mM, pH8.5), and the ratio of dopamine to the Tris·HCl aqueous solution is 0.01g:5mL. After 8 hours of treatment, it is taken out, washed with deionized water, and dried with N2 to obtain a treated body 2 for standby use.
[0030] A third treatment liquid is applied to the surface of the treatment body 2 to form a coating layer. The raw materials of the third treatment liquid are TiB2, fluorinated graphene, CNT, epoxy resin, and diluent = 35:30:2:30:3. The diluent is diethylenetriamine. CNT is copper-plated CNT. After weighing the above raw materials in proportion, they are evenly mixed to obtain the third treatment liquid. The coating thickness is 5mm. The coating layer is first left at room temperature for 20 hours, and then placed in a heating furnace for heating treatment. First, the temperature is increased to 100°C at a rate of 20°C / h and maintained for 2 hours, and then the temperature is increased to 150°C at a rate of 20°C / h and maintained for 2 hours; then, the temperature is increased to 200°C at a rate of 25°C, to 400°C at a rate of 20°C / h, to 600°C at a rate of 20°C / h, and to 900°C at a rate of 20°C / h, and kept warm for 8 hours. After the heat preservation is completed, the material is naturally cooled to room temperature to obtain a cathode material for aluminum electrolysis.
[0031] Example 2
[0032] The difference between this embodiment and embodiment 1 is that the third treatment liquid is different. The raw materials of the third treatment liquid are TiB2, fluorinated graphene, CNT, epoxy resin, and diluent = 38:30:2:32:3.
[0033] Example 3
[0034] The difference between this embodiment and embodiment 1 is that the CNT can be made of CNT material.
[0035] Comparative Example 1
[0036] The difference between this comparative example and Example 1 is that the fluorinated graphene is replaced by TiB2 and CNT is not added.
[0037] Comparative Example 2
[0038] The difference between this comparative example and Example 1 is that the base material is not pretreated, and the third treatment liquid is directly coated on the surface of the base material.
[0039] Comparative Example 3
[0040] The difference between this comparative example and Example 1 is that the temperature is increased to 200°C at a rate of 25°C, to 400°C at a rate of 20°C / h, to 600°C at a rate of 20°C / h, to 900°C at a rate of 20°C / h, and kept warm for 8h.
[0041] Test example
[0042] Using Examples 1-3 and Comparative Examples 1-3 as test samples, the coating properties were measured, and the results are shown in Table 1. The test indicators include coating tensile strength (refer to GB8721-88), coating adhesion strength (refer to GB8721-88), and coating resistivity (using a four-probe method, room temperature).
[0043] Table 1 Measurement results
[0044]
[0045] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a cathode material for aluminum electrolysis, characterized in that: The steps include: After the base material is pretreated, a transition layer and a coating layer are sequentially arranged on the surface thereof; The raw material components of the coating layer include TiB2, fluorinated graphene, CNT, epoxy resin and diluent.
2. The method for preparing a cathode material for aluminum electrolysis according to claim 1, characterized in that: The pretreatment is as follows: after the base material is cleaned, it is immersed in an acidic solution, taken out after 30 minutes, and dried with N2; the acidic solution is a mixture of concentrated sulfuric acid and hydrogen peroxide, and the volume ratio of concentrated sulfuric acid to hydrogen peroxide is 7:
3.
3. The method for preparing a cathode material for aluminum electrolysis according to claim 1, characterized in that: The diluent includes at least one of ethylene glycol and diethylenetriamine.
4. The method for preparing a cathode material for aluminum electrolysis according to claim 1, characterized in that: The ratio of TiB2, fluorinated graphene, CNT, epoxy resin and diluent is 30-50:15-40:1-5:20-35:1-5.
5. The method for preparing a cathode material for aluminum electrolysis according to claim 1, characterized in that: The CNTs are copper-plated CNTs.
6. The method for preparing a cathode material for aluminum electrolysis according to any one of claims 1 to 5, characterized in that: The preparation method of the transition layer is as follows: placing the pretreated substrate material in a first treatment liquid, and after treatment, obtaining a treatment body 1; the treatment liquid 1 is obtained by dissolving (3-aminopropyl)triethoxysilane in a solvent; immersing the treatment body 1 in a second treatment liquid, and after treatment, obtaining a treatment body 2 for standby use; the second treatment liquid is obtained by dissolving dopamine in a Tris·HCl aqueous solution.
7. The method for preparing a cathode material for aluminum electrolysis according to claim 6, characterized in that: The solvent is V (acetone): V (water) = 5:
1.
8. The method for preparing a cathode material for aluminum electrolysis according to claim 6, characterized in that: The ratio of dopamine to Tris·HCl aqueous solution is 0.01 g:2.5-10 mL.
9. The method for preparing a cathode material for aluminum electrolysis according to any one of claims 1 to 5, characterized in that: The coating layer is cured: the coating layer is first allowed to stand at room temperature for 18 to 30 hours, and then placed in a heating furnace for heating treatment, first heating to 100°C at a rate of 20°C / h and holding for 1 to 3 hours, and then heating to 150°C at a rate of 20°C / h and holding for 1 to 3 hours; then, heating to 200°C at a rate of 25°C, heating to 400°C at a rate of 20°C / h, heating to 600°C at a rate of 20°C / h, and heating to 900°C at a rate of 20°C / h, and keeping warm for 8 to 10 hours.
10. A cathode material obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Wettable cathode material for aluminum electrolytic cell as well as preparation method and application thereof
CN110219022A
TiB2-graphene composite cathode material for aluminum electrolysis and preparation method thereof
CN110436933A
Normal temperature solidified titanium boride cathode coating for aluminium electrolysis
CN1537974A
Titanium boride / aluminium oxide cathode coating for aluminium electrolysis and its preparation method
CN1537975A
Nanotube-containing composite bodies, and methods for making same
US20060062985A1