Method for regulating and controlling thickness of AgCl film layer on surface of chloride ion selective electrode
Through pulse current anodizing and multi-step pretreatment technology, the problem of poor thickness uniformity of AgCl film layer is solved, high reproducibility and good potential response are achieved, and probe life is extended.
Patent Information
- Application Number
- CN202410988070.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The AgCl film layer thickness uniformity of the existing chloride ion selective electrodes is poor, and the reproducibility is average, which affects the life of the probe.
The pulse current anodization method is adopted to control the thickness of the AgCl film layer by adjusting the current density, duty cycle, polarization time and pulse frequency, and the uniformity and performance of the film layer are improved by using epoxy resin sealing welding and multi-step pretreatment.
The uniformity and potential reproducibility of the AgCl film layer thickness are achieved, the potential response curve to chloride ion concentration is good, and the theoretical and actual film layer thickness error can be controlled within 10 microns, which extends the probe life.
Smart Images

Figure CN118932468A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to a film thickness control method, in particular to a method for controlling the thickness of an AgCl film layer on the surface of a chloride ion selective electrode. Background Art
[0002] Currently, the more commonly used method for making chloride ion selective electrodes (i.e., AgCl electrodes) is to pass a constant current in an HCl solution for anodic chlorination, that is, to form a layer of AgCl film on the surface of the silver wire with poor thickness uniformity. The Ag / AgCl electrode prepared by this method has general reproducibility, and the prepared probe anodized film is thin, which affects the life of the probe. Summary of the invention
[0003] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a method for regulating the thickness of the AgCl film layer on the surface of a chloride ion selective electrode with good reproducibility, high accuracy and uniform thickness.
[0004] Technical solution: The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode described in the present invention comprises the following steps:
[0005] Step 1, welding one end of the silver wire to the copper wire, sealing the welding point, and then pre-treating the exposed silver wire to be polarized;
[0006] Step 2: The polarization system is Ag / AgCl electrode-silver wire to be polarized-graphite cylinder, HCl solution is used as electrolyte, and the pretreated silver wire to be polarized is placed in the system;
[0007] Step 3, adjusting the pulse current parameters, including current density, duty cycle, polarization time, and pulse frequency, to perform pulse current anodic chlorination on the pretreated silver wire to form a dense AgCl film layer on the surface;
[0008] The thickness of the AgCl film satisfies the following relationship:
[0009] d=|-12.9066-87.619x1+38.463x2+2.728x3+0.01258x4|
[0010] Among them, d is the theoretical film thickness, x1 is the current density, x2 is the duty cycle, x3 is the polarization time, and x4 is the pulse frequency.
[0011] Furthermore, in step 1, any one of epoxy resin, polyurea-formaldehyde resin, and polyimide resin is used for the sealing welding, preferably epoxy resin. The pretreatment is to polish the silver wire with sandpaper, put it in acetone for ultrasonic vibration for degreasing, soak it in NH4OH, rinse it with distilled water, soak it in concentrated nitric acid, and rinse it with distilled water. The length of the exposed silver wire to be polarized is 8 to 12 mm and the diameter is 1 to 2 mm.
[0012] Furthermore, in step 2, the outer diameter of the graphite tube is 65-70 mm, the inner diameter is 55-60 mm, the height is 60-70 mm, and a plurality of small holes are evenly arranged on the side. The concentration of the HCl solution is 0.1-0.3 mol / L. The pH is 1-3, preferably, pH=1.
[0013] Furthermore, the pulse current density is 0.1-0.4 mA / cm 2 The current duty cycle is 40% to 80%. The anodic chlorination time is 6 to 18 hours. The pulse frequency is 10 Hz to 1000 Hz.
[0014] The current parameters have a significant impact on the film structure and performance, and the current parameters mainly include current density, duty cycle, polarization time, pulse frequency, etc. The optimization of current parameters can improve the thickness of the AgCl film on the surface of the silver substrate, making it more practical.
[0015] There are two ways to apply current: constant current and pulse current. Pulse current anodization current is applied discontinuously, which provides time for heat dissipation during the oxidation process. Compared with constant current polarization, it increases the cooling time, and the duty cycle of the current and the frequency of the pulse current can be adjusted, making the reaction process relatively stable, so the treatment process and film performance are more controllable.
[0016] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0017] 1. The operation process is simple, the thickness of the Ag / AgCl electrode film produced is uniform, the potential reproducibility is good, and the response curve of the potential to the chloride ion concentration is good;
[0018] 2. The problem of thin AgCl film layer prepared by constant current can be overcome. The present invention adjusts the parameters of pulse current to produce AgCl film layer of corresponding thickness. The error between theoretical film layer thickness and actual film layer thickness can be accurately controlled within the range of 10 microns. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a diagram of the Ag / AgCl electrode polarization device of the present invention;
[0020] Figure 2 Electron microscope images of the Ag / AgCl electrode film thickness under different current application modes, where (a) is pulse current and (b) is constant current;
[0021] Figure 3 This is the relationship curve between the Ag / AgCl electrode potential and the chloride ion concentration in the simulated pore fluid of concrete. Figure 3In the graph, the horizontal axis is the chloride ion concentration, the vertical axis is the potential, and the slope is 54mV / decade;
[0022] Figure 4 Electron micrographs of the Ag / AgCl electrode surface under different current application modes, where (a) is pulse current and (b) is constant current;
[0023] Figure 5 Nquist diagram of the EIS curve fitting diagram of the Ag / AgCl electrode under different current application modes;
[0024] Figure 6 Bode diagram of the EIS curve fitting diagram of the Ag / AgCl electrode under different current application methods. DETAILED DESCRIPTION
[0025] In the following examples, the materials, reagents, instruments, etc. used are all commercially available unless otherwise specified. Experimental methods without specific conditions in the examples are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0026] The interaction between electrical parameters is not considered in the process of studying the film performance, so the four-factor three-level orthogonal test table L9 (3 4 ) was used to design the experimental scheme, and the specific factor level combinations are shown in Table 1.
[0027] Table 1 Orthogonal test factor level table
[0028]
[0029] The current density, duty cycle, polarization time, and pulse frequency are represented by letters A, B, C, and D, respectively, and filled in L9(3 4 ) In the orthogonal test table, the test scheme is shown in Table 2. According to the requirements of the above two test schemes, the test is carried out with various factors. After the test, the sample is removed and repeatedly washed with deionized water to completely remove the electrolyte remaining on the surface of the sample to avoid affecting the accuracy of subsequent detection.
[0030] Table 2 Orthogonal test plan
[0031] Example A B C D Trial plan 1 0.1 40 6 10 <![CDATA[A1B1C1D1]]> 2 0.1 60 18 100 <![CDATA[A1B2C3D2]]> 3 0.1 80 12 1000 <![CDATA[A1B3C2D3]]> 4 0.2 40 18 1000 <![CDATA[A2B1C3D3]]> 5 0.2 60 12 10 <![CDATA[A2B2C2D1]]> 6 0.2 80 6 100 <![CDATA[A2B3C1D2]]> 7 0.4 40 12 100 <![CDATA[A3B1C2D2]]> 8 0.4 60 6 1000 <![CDATA[A3B2C1D3]]> 9 0.4 80 18 10 <![CDATA[A3B3C3D1]]>
[0032] Example 1
[0033] A pulse anodizing preparation method for regulating the thickness of an AgCl film layer on the surface of a chloride ion selective electrode comprises the following steps:
[0034] (1) Weld one end of a silver wire (1 mm in diameter and 15 mm in length) to a copper conductor and seal the weld with epoxy resin. Then pretreat the exposed 10 mm long silver wire to be polarized by polishing it with 400# sandpaper, 1000# sandpaper, and 1200# sandpaper in sequence. Then, degrease the silver wire by ultrasonic vibration in acetone for 15 min, soak it in 28% NH4OH (25 ml of deionized water + 9.7 ml of ammonia water) for 4 h, rinse it with distilled water, soak it in concentrated nitric acid for 1 min, and rinse it with distilled water.
[0035] (2) The polarization system is Ag / AgCl electrode-silver wire to be polarized-graphite cylinder, with 0.1 mol / L HCl solution as the electrolyte, and the silver wire to be polarized is placed in the system. The graphite cylinder has an outer diameter of 70 mm, an inner diameter of 60 mm, and a height of 70 mm, and small holes are evenly drilled on the side.
[0036] (3) Adjust the pulse current parameters and the current density to 0.1 mA / cm 2 , the current duty cycle is 40%, the anodic chlorination time is 6h, the pulse frequency is 10Hz, the pH of the solution is 1, and the pretreated silver wire is Figure 1 Pulse current anodic chlorination is carried out in the device shown, and a dense AgCl film layer with a thickness of 10.3 μm is formed on the surface.
[0037] Example 2
[0038] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.1 mA / cm 2 , the current duty cycle is 60%, the anodic chlorination time is 18h, the pulse frequency is 100Hz, and the thickness of the obtained AgCl film is 50.9μm.
[0039] Example 3
[0040] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.1 mA / cm 2 , the current duty cycle is 80%, the anodic chlorination time is 12h, the pulse frequency is 1000Hz, and the obtained AgCl film thickness is 78.3μm.
[0041] Example 4
[0042] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.2 mA / cm 2 , the current duty cycle is 40%, the anodic chlorination time is 18h, the pulse frequency is 1000Hz, and the thickness of the obtained AgCl film is 15.6μm.
[0043] Example 5
[0044] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.2 mA / cm 2 , the current duty cycle is 60%, the anodic chlorination time is 12h, the pulse frequency is 10Hz, and the thickness of the obtained AgCl film is 27.6μm.
[0045] Example 6
[0046] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.2 mA / cm 2 , the current duty cycle is 80%, the anodic chlorination time is 6h, the pulse frequency is 100Hz, and the thickness of the obtained AgCl film is 12.3μm.
[0047] Example 7
[0048] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.4 mA / cm 2 , the current duty cycle is 40%, the anodic chlorination time is 12h, the pulse frequency is 100Hz, and the obtained AgCl film thickness is 16.2μm.
[0049] Example 8
[0050] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.4 mA / cm 2 , the current duty cycle is 60%, the anodic chlorination time is 6h, the pulse frequency is 1000Hz, and the thickness of the obtained AgCl film is 12.6μm.
[0051] Example 9
[0052] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.4 mA / cm 2 , the current duty cycle is 80%, the anodic chlorination time is 18h, the pulse frequency is 10Hz, and the thickness of the obtained AgCl film is 20.3μm.
[0053] Table 3 Thickness of AgCl film obtained in Examples 1 to 9
[0054] Example Film thickness 1 10.3μm 2 50.9μm 3 78.3μm 4 15.6μm 5 27.6μm 6 12.3μm 7 16.2μm 8 12.6μm 9 20.3μm
[0055] Example 10
[0056] In order to more accurately control the film thickness by adjusting the electrical parameters, a multivariate linear regression equation for the film thickness was established based on the results of 9 orthogonal tests:
[0057]
[0058]
[0059] The solution is: a=-12.9066, b1=-87.619, b2=38.463, b3=2.728, b4=0.01258.
[0060] That is, the regression equation is:
[0061] y=-12.9066-87.619x1+38.463x2+2.728x3+0.01258x4
[0062] Since the film thickness is ≥ 0, the equation is optimized to obtain the relationship between the film thickness d:
[0063] d=|-12.9066-87.619x1+38.463x2+2.728x3+0.01258x4|
[0064] Among them, x1 is the current density, x2 is the duty cycle, x3 is the polarization time, and x4 is the pulse frequency.
[0065] Embodiment 11
[0066] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the current density is 0.1 mA / cm 2 , the current duty cycle is 80%, the anodic chlorination time is 16h, and the pulse frequency is 1000Hz.
[0067] Substituting into the formula obtained in Example 10, the theoretical film thickness d = 65.3 μm is calculated. Figure 2 As shown, the actual film thickness D = 72.3 μm, Dd = 7.0 μm < 10 μm.
[0068] Example 12
[0069] The remaining steps of this embodiment are the same as those of embodiment 1, except that in step (3), the pulse current density is 0.2 mA / cm 2 , the duty cycle is 60%, the polarization time is 7.5h, and the pulse frequency is 10Hz.
[0070] Substituting the formula obtained in Example 10, the theoretical film thickness d=13.2 μm is calculated. The actual film thickness D=14.0 μm, Dd=0.8 μm<10 μm.
[0071] The color of the electrode surface is uniform. The thickness of the film layer is measured at five random points. The results are shown in Table 4 below. The thickness ranges from 13.7 to 14.2 μm, indicating that the thickness of the formed film layer is uniform.
[0072] serial number 1 2 3 4 5 Film thickness (μm) 14.2 13.7 14.1 14.0 13.9
[0073] Embodiment 13
[0074] The electrode prepared in Example 1 was selected to test the electrode potential in concrete simulation liquid with chloride ion contents of (0.005 mol / L, 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.5 mol / L, 1 mol / L) respectively.
[0075] Fitting result: E = 23.925-54.243lg [Cl - ]
[0076] like Figure 3 As shown, the slope of the response curve of the electrode potential and the log value of the chloride ion concentration is around 54mV / decade, which has a good linear relationship.
[0077] Comparative Example 1
[0078] A constant current preparation method for an AgCl film layer comprises the following steps:
[0079] (1) Weld one end of a silver wire (1 mm in diameter and 15 mm in length) to a copper conductor and seal the weld with epoxy resin. Then pretreat the exposed 10 mm long silver wire to be polarized by polishing it with 400# sandpaper, 1000# sandpaper, and 1200# sandpaper in sequence. Then, degrease the silver wire by ultrasonic vibration in acetone for 15 min, soak it in 28% NH4OH (25 ml of deionized water + 9.7 ml of ammonia water) for 4 h, rinse it with distilled water, soak it in concentrated nitric acid for 1 min, and rinse it with distilled water.
[0080] (2) The polarization system is Ag / AgCl electrode-silver wire to be polarized-graphite cylinder, with 0.1 mol / L HCl solution as the electrolyte, and the silver wire to be polarized is placed in the system. The graphite cylinder has an outer diameter of 70 mm, an inner diameter of 60 mm, and a height of 70 mm, and small holes are evenly drilled on the side.
[0081] (3) Current density is 0.1 mA / cm 2 , the anodic chlorination time is 6h, the pH value of the solution is 1, and the pretreated silver wire is Figure 1 Constant current anodic chlorination is carried out in the apparatus shown.
[0082] like Figure 4 The surface of the film layer prepared by pulse current anodization is more uniform and dense, and has higher flatness, which is better than the film layer prepared by constant current anodization.
[0083] Table 5 EIS curve fitting table of Ag / AgCl probe
[0084] Pulse current Constant current <![CDATA[R s / (Ω·cm 2 )]]> 2.072 2.227 <![CDATA[Q c / (F·cm 2 )]]> <![CDATA[5.502×10 -4 ]]> <![CDATA[4.668×10 -4 ]]> <![CDATA[n1]]> 0.5586 0.5718 <![CDATA[R c / (Ω·cm 2 )]]> 2713 22.83 <![CDATA[Q dl / (F·cm 2 )]]> <![CDATA[1.388×10 -2 ]]> <![CDATA[2.03×10 -5 ]]> <![CDATA[n2]]> 0.7975 0.9195 <![CDATA[R ct / (Ω·cm 2 )]]> 2407 6037
[0085] Figures 5-6 The EIS curve fitting diagram of the Ag / AgCl electrode under different current application modes. It can be seen that the film layer of pulse current anodization has a larger R c Because AgCl has poor conductivity, the thicker the AgCl film on the surface, the greater the internal resistance, which means that the film layer of pulse current anodization is thicker. And the film layer of pulse current anodization has a smaller R ct and a larger Q dl , which means that the reversible redox transformation on the Ag / AgCl surface is easier to carry out. The specific data comparison is shown in Table 5 above.
Claims
1. A method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode, characterized in that: The following steps are involved: Step 1, welding one end of the silver wire to the copper wire, sealing the welding point, and then pre-treating the exposed silver wire to be polarized; Step 2: The polarization system is Ag / AgCl electrode-silver wire to be polarized-graphite cylinder, HCl solution is used as electrolyte, and the pretreated silver wire to be polarized is placed in the system; Step 3, adjusting the pulse current parameters, including current density, duty cycle, polarization time, and pulse frequency, to perform pulse current anodic chlorination on the pretreated silver wire to form a dense AgCl film layer on the surface; The thickness of the AgCl film layer satisfies the following relationship: d=|-12.9066-87.619x1+38.463x2+2.728x3+0.01258x4| Among them, d is the theoretical film thickness, x1 is the current density, x2 is the duty cycle, x3 is the polarization time, and x4 is the pulse frequency.
2. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: In the step 1, any one of epoxy resin, polyurea-formaldehyde resin and polyimide resin is used for sealing the welding point.
3. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: In the step 1, the pretreatment is to polish the silver wire with sandpaper, put it in acetone for ultrasonic vibration for degreasing, soak it in NH4OH, rinse it with distilled water, soak it in concentrated nitric acid, and rinse it with distilled water.
4. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: In the step 1, the length of the exposed silver wire to be polarized is 8 to 12 mm, and the diameter is 1 to 2 mm.
5. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: In the step 2, the outer diameter of the graphite cylinder is 65-70 mm, the inner diameter is 55-60 mm, the height is 60-70 mm, and a plurality of small holes are evenly arranged on the side.
6. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: In the step 2, the concentration of the HCl solution is 0.1-0.3 mol / L.
7. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: The pulse current density is 0.1-0.4 mA / cm 2 .
8. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: The current duty cycle is 40% to 80%.
9. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: The anodic chlorination time is 6 to 18 hours.
10. The method for controlling the thickness of the AgCl film layer on the surface of a chloride ion selective electrode according to claim 1, characterized in that: The pulse frequency is 10 Hz to 1000 Hz.