Method for preparing skin-friendly antibacterial fiber by recycling waste polyester

Through the pretreatment, decomposition, additive mixing and melt spinning process of waste polyester, combined with microwave-assisted heating, high-quality skin-friendly and antibacterial fibers are prepared, which solves the problem that fibers in the prior art are difficult to take into account both skin-friendly and antibacterial properties. , achieving efficient recycling and performance improvement, reducing resource waste and health risks.

CN118932538APending Publication Date: 2024-11-12JIANGSU GEM ADVANCED FIBER MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411176140.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing waste polyester recycling and recycled fiber products are difficult to take into account both skin-friendly and antibacterial properties, resulting in health risks and waste of resources in the fields of medical care, hygiene and sports.

Method used

Use waste polyester pretreatment, impurity removal, additive mixing, melt spinning and multi-stage stretching processes, combined with microwave-assisted heating to prepare high-quality skin-friendly and antibacterial fibers, and improve the performance of the fibers by adding antibacterial compounds and antistatic agents. .

Benefits of technology

It realizes efficient recycling of used polyester, improves the skin-friendly comfort and antibacterial properties of fibers, reduces bacterial growth risks, reduces resource waste, simplifies production processes, and reduces costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of antibacterial fibers, and discloses a method for preparing skin-friendly antibacterial fibers by recycling waste polyester, which comprises the following steps: S1, pretreatment of waste polyester: sorting waste polyester, removing impurities, cleaning and drying; s2, impurity removal: dissolving in a composite solvent, and performing nitrogen protection to obtain high-quality polyester; s3, additive mixing: adding a skin-friendly agent, an antibacterial compound and an antistatic agent; s4, spinning: performing melt spinning in a melt spinning machine to form nascent fibers; and S5, post-treatment: carrying out multi-stage stretching, segmented temperature control and microwave-assisted heat setting. According to the performance indexes of the skin-friendly antibacterial fiber, the fiber fineness ranges from 0.5 dtex to 3 dtex, the breaking strength ranges from 3.5 cN / dtex to 5.5 cN / dtex, the antibacterial rate reaches 95% or above, the skin-friendly performance is measured according to the skin moisture content increasing rate by 20% or above, and the good antistatic performance is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antibacterial fibers, and in particular to a method for preparing skin-friendly antibacterial fibers by recycling and regenerating waste polyester. Background Art

[0002] With the rapid development of the textile industry, polyester fiber has been widely used in clothing, home textiles and other fields due to its excellent properties, such as high strength, good wrinkle resistance and dimensional stability. However, a large number of polyester products are discarded after use, which not only causes a waste of resources, but also puts great pressure on the environment.

[0003] In recent years, the increasing awareness of environmental protection has prompted people to seek effective ways to recycle waste polyester. Traditional methods of recycling waste polyester often have technical limitations, such as complex recycling process, high cost, and poor quality of regenerated fibers.

[0004] In the application of fiber materials, consumers have increasing requirements for comfort and health. Skin-friendly performance has become an important consideration for fiber products, which can reduce skin irritation and provide a better wearing experience. At the same time, antibacterial properties have also received widespread attention, especially in the fields of medical care, hygiene and sports. Fibers with antibacterial functions can effectively reduce bacterial growth and protect the health of users.

[0005] The existing regenerated fiber products on the market often have difficulty in achieving both skin-friendly and antibacterial properties, or their performance is not ideal. Therefore, developing an innovative method for recycling waste polyester to produce fibers with both good skin-friendly properties and high antibacterial properties has become a technical problem and an important research direction that needs to be solved in the current textile field. Summary of the invention

[0006] 1. Technical issues to be solved

[0007] In view of the shortcomings of the prior art, the present invention provides a method for recycling waste polyester to prepare skin-friendly and antibacterial fibers.

[0008] (II) Technical solution

[0009] A method for recycling and regenerating waste polyester to prepare skin-friendly antibacterial fiber, comprising the following steps:

[0010] S1. Pretreatment of waste polyester: sort the waste polyester to remove non-polyester components and polyester materials that are severely damaged or stained with stubborn stains, then perform deep cleaning and finally dry to ensure that the moisture content of the waste polyester is less than 5%;

[0011] S2, impurity removal: the pretreated waste polyester is placed in a composite solvent, stirred continuously for 30 to 60 minutes at a stirring speed of 300 to 500 r / min, and inert gas nitrogen is introduced to protect the solution to prevent oxidation, and high-quality polyester is obtained by filtering;

[0012] S3, additive mixing: drying and crushing the polyester in S2, adding a skin-friendly agent, an antibacterial compound and an antistatic agent thereto to obtain a mixed raw material;

[0013] S4, spinning: the dried mixed raw material is subjected to secondary drying, and melt-spinning is performed in a melt spinning machine to form primary fibers;

[0014] S5. Post-treatment: The nascent fiber is subjected to multi-stage stretching, and segmented temperature control is adopted during the stretching process, and then heat setting is performed. Microwave-assisted heating is adopted during heat setting. The power of microwave-assisted heating is 800-1200W, and the heating time is 10-15min, so that the internal structure of the fiber is more stable, and skin-friendly and antibacterial fiber is obtained.

[0015] Preferably, the deep cleaning in step S1 includes ultrasonic cleaning and chemical cleaning, and the cleaning agent used in the chemical cleaning is a sodium carbonate solution with a mass concentration of 5-10%.

[0016] Preferably, the composite solvent in step S2 is dimethylformamide and dimethyl sulfoxide in a mass ratio of 1:0.8-1.2.

[0017] Preferably, the skin-friendly agent in step S3 is sodium hyaluronate having a natural moisturizing factor, and the amount of the skin-friendly agent added is 8-12% of the mass of the polyester.

[0018] Preferably, the melt temperature of the melt spinning process in step S4 is 230-280° C., and the spinneret hole diameter is 0.15-0.35 mm.

[0019] Preferably, the number of multi-stage stretching in step S5 is 2, and the stretching multiple of each stage is 1.2-2.5; the segmented temperature control is 3 stages, stage 1 is 70-100°C, stage 2 is 110-150°C, and stage 3 is 140-200°C.

[0020] Preferably, the preparation method of the antibacterial compound and the antistatic agent in step (1) is as follows:

[0021] (1) dissolving maleic anhydride in anhydrous ethanol to prepare a solution, adding guanidine hydrochloride and stirring, passing nitrogen for 30 to 40 minutes, stirring and reacting in a water bath at 60 to 80° C. for 3 to 8 hours to obtain functionalized maleic anhydride;

[0022] (2) dissolving functionalized maleic anhydride in anhydrous ethanol, adding 2,3-epoxypropyltrimethylammonium chloride thereto, stirring evenly, adding a catalyst stannous octoate, reacting for 1 to 3 hours, and obtaining a reaction solution; adding 2-vinylimidazole to anhydrous ethanol, stirring to dissolve, and then mixing with the reaction solution, adding 2% by mass of azobisisobutyronitrile, and reacting in a constant temperature water bath at 80 to 100° C. for 5 to 10 hours, and after the reaction is completed, precipitating with distilled water, and drying in a vacuum drying oven at 60 to 80° C. for 10 to 20 hours to obtain an antibacterial compound;

[0023] (3) dissolving chitosan in a 10% by mass glacial acetic acid solution to prepare a chitosan solution, then dissolving acrylamide in water to prepare an acrylamide solution, heating the chitosan to 50-60° C. and adding it to the acrylamide solution, adding an initiator, ammonium persulfate, heating to 80-100° C. to react for 2-6 hours, and drying to obtain a grafted product;

[0024] (4) slowly dripping diethylenetriamine into the ethyl acrylate and methanol solution under nitrogen protection, reacting for 2 to 5 hours, removing methanol under reduced pressure, heating to 120 to 150° C. and reacting under reduced pressure for 3 to 6 hours, adding water and stirring evenly after the reaction, adding 2-epoxypropyl dodecyl dimethyl quaternary ammonium salt, stirring and reacting at 60 to 80° C. for 10 to 30 minutes, adding acetone for precipitation and separation, and vacuum drying to obtain a modified quaternary ammonium salt;

[0025] (5) The modified quaternary ammonium salt, the grafted product, anhydrous ethanol, and the initiator benzoyl peroxide are mixed, stirred and reacted at 60 to 80° C. for 6 to 10 hours, and dried after the reaction to obtain an antistatic agent.

[0026] 8. The method for preparing skin-friendly and antibacterial fiber by recycling and regenerating waste polyester according to claim 7, characterized in that: in the step (1), the mass ratio of maleic anhydride to guanidine hydrochloride is 1:0.6-0.8; in the step (2), the mass ratio of functionalized maleic anhydride, 2,3-epoxypropyltrimethylammonium chloride, stannous octoate, 2-vinylimidazole, and 2% azobisisobutyronitrile is 1:0.2-0.5:0.05-0.08:0.5-0.8:0.05-0.1.

[0027] Preferably, in the step (3), the mass ratio of chitosan, acrylamide and initiator ammonium persulfate is 1:0.6-0.8:0.1-0.3; in the step (4), the mass ratio of diethylenetriamine, ethyl acrylate and 2-epoxypropyl dodecyl dimethyl ammonium salt is 1:1.2-1.5:0.4-0.8; in the step (5), the mass ratio of modified quaternary ammonium salt, grafted product and initiator benzoyl peroxide is 1:5-7:0.1-0.3.

[0028] Preferably, the skin-friendly antibacterial fiber is used in the fields of automotive apparel, home textiles, clothing, and building materials.

[0029] (III) Beneficial technical effects

[0030] The performance indicators of skin-friendly antibacterial fibers include fiber fineness of 0.5-3dtex, breaking strength of 3.5-5.5cN / dtex, antibacterial rate of more than 95%, skin-friendly performance measured by skin moisture content increase rate of more than 20%, and good antistatic performance.

[0031] The method for preparing skin-friendly and antibacterial fibers by recycling and regenerating waste polyester provided by the present invention has many significant beneficial effects.

[0032] First of all, it realizes the efficient recycling of waste polyester, reduces resource waste and environmental pollution, and conforms to the concept of sustainable development. Through innovative recycling technology, the utilization rate of waste polyester is improved and the demand for new raw materials is reduced.

[0033] In terms of skin-friendly performance, the prepared fiber can significantly improve the comfort of contact with the skin, reduce friction and irritation to the skin, make the wearer feel softer and more comfortable, and is especially suitable for people with sensitive skin.

[0034] The improvement of antibacterial properties effectively inhibits the growth of bacteria and microorganisms. When used in medical, hygiene and sports fields, it reduces the risk of infection and protects the health of users.

[0035] The fibers prepared by this method have excellent physical properties, such as high strength and good dimensional stability, ensuring the durability and reliability of the fibers during use.

[0036] In addition, the innovative preparation process is relatively simple, easy to operate and control, and is conducive to large-scale industrial production. At the same time, it reduces production costs, improves production efficiency, and has good economic benefits and market competitiveness.

[0037] In summary, the present invention not only solves the problem of recycling waste polyester, but also provides a high-performance, multifunctional new product for the fiber material market, which has broad application prospects and important social value. DETAILED DESCRIPTION

[0038] Example 1

[0039] S1. Pretreatment of waste polyester: sort the waste polyester to remove non-polyester components and polyester materials that are severely damaged or stained with stubborn stains. Then perform deep cleaning, including ultrasonic cleaning and chemical cleaning, to remove fine impurities and residual stains. The cleaning agent used for chemical cleaning is sodium carbonate solution with a mass concentration of 5%. Finally, dry it to ensure that the moisture content of the waste polyester is less than 5%.

[0040] S2. Impurity removal: The pretreated waste polyester is placed in a composite solvent containing dimethylformamide and dimethyl sulfoxide in a mass ratio of 1:0.8, and stirred continuously for 30 minutes at a stirring speed of 300 r / min. At the same time, inert gas nitrogen is introduced for protection to prevent oxidation of the solution, and high-quality polyester is obtained by filtration.

[0041] S3, additive mixing: the polyester in S2 is dried and crushed, and a skin-friendly agent, an antibacterial compound and an antistatic agent are added thereto. The skin-friendly agent is sodium hyaluronate with a natural moisturizing factor, and the amount of the skin-friendly agent added is 8% of the mass of the polyester to obtain a mixed raw material.

[0042] S4. Spinning: The dried mixed raw materials are dried for a second time and melt-spun in a melt spinning machine with a melt temperature of 230° C. and a spinneret diameter of 0.15 mm to form primary fibers.

[0043] S5. Post-treatment: The spun fibers are subjected to multi-stage stretching. During the stretching process, segmented temperature control is adopted. The number of multi-stage stretching is 2, and the stretching multiple of each stage is 1.2. The segmented temperature control is 3 sections, with the first section being 70°C, the second section being 110°C, and the third section being 140°C. Then, heat setting is performed. Microwave-assisted heating is adopted during heat setting. The power of microwave-assisted heating is 800 W, and the heating time is 10 minutes, so that the internal structure of the fiber is more stable, and skin-friendly and antibacterial fibers are obtained.

[0044] The preparation method of the antibacterial compound is as follows:

[0045] (1) 20 g of maleic anhydride was dissolved in 120 mL of anhydrous ethanol to prepare a solution, 12 g of guanidine hydrochloride was added and stirred, nitrogen was passed through for 30 min, and the mixture was stirred in a 60° C. water bath for 3 h to obtain functionalized maleic anhydride;

[0046] (2) 30 g of functionalized maleic anhydride was dissolved in 150 mL of anhydrous ethanol, 6 g of 2,3-epoxypropyltrimethylammonium chloride was added thereto, the mixture was stirred evenly, 1.5 g of catalyst stannous octoate was added, and the mixture was reacted for 1 h to obtain a reaction solution; 15 g of 2-vinylimidazole was added to 150 mL of anhydrous ethanol, stirred to dissolve, and then mixed with the reaction solution, 1.5 g of 2% azobisisobutyronitrile was added, and the mixture was reacted in a constant temperature water bath at 80 ° C for 5 h. After the reaction was completed, the mixture was precipitated with distilled water and dried in a vacuum drying oven at 60 ° C for 10 h to obtain an antibacterial compound.

[0047] The preparation method of the antistatic agent is as follows:

[0048] (3) 100 g of chitosan was dissolved in 1000 mL of 10% glacial acetic acid solution to prepare a chitosan solution, and 60 g of acrylamide was dissolved in 500 mL of water to prepare an acrylamide solution. The chitosan was heated to 50° C. and then added to the acrylamide solution. 10 g of initiator ammonium persulfate was added, the temperature was raised to 80° C. for reaction for 2 h, and then dried to obtain a grafted product.

[0049] (4) 10 g of diethylenetriamine was slowly dripped into 10 g of ethyl acrylate and 50 mL of methanol solution under nitrogen protection, and the reaction was carried out for 2 h. The methanol was removed under reduced pressure, and the temperature was raised to 120° C. and the reaction was carried out under reduced pressure for 3 h. After the reaction was completed, water was added and stirred evenly. 4 g of 2-epoxypropyl dodecyl dimethyl quaternary ammonium salt was added thereto, and the reaction was stirred at 60° C. for 10 min. Acetone was added for precipitation and separation, and vacuum drying was performed to obtain a modified quaternary ammonium salt;

[0050] (5) 10 g of modified quaternary ammonium salt, 60 g of grafted product, 200 mL of anhydrous ethanol, and 1 g of initiator benzoyl peroxide were mixed, stirred and reacted at 60° C. for 6 h, and dried after the reaction to obtain an antistatic agent.

[0051] Example 2

[0052] S1. Pretreatment of waste polyester: sort the waste polyester to remove non-polyester components and polyester materials that are severely damaged or stained with stubborn stains. Then perform deep cleaning, including ultrasonic cleaning and chemical cleaning, to remove fine impurities and residual stains. The cleaning agent used for chemical cleaning is sodium carbonate solution with a mass concentration of 10%. Finally, dry it to ensure that the moisture content of the waste polyester is less than 5%.

[0053] S2. Impurity removal: The pretreated waste polyester is placed in a composite solvent containing dimethylformamide and dimethyl sulfoxide in a mass ratio of 1:1.2, and stirred continuously for 60 minutes at a stirring speed of 500 r / min. At the same time, inert gas nitrogen is introduced for protection to prevent oxidation of the solution, and high-quality polyester is obtained by filtration.

[0054] S3, additive mixing: the polyester in S2 is dried and crushed, and a skin-friendly agent, an antibacterial compound and an antistatic agent are added thereto. The skin-friendly agent is sodium hyaluronate with a natural moisturizing factor, and the amount of the skin-friendly agent added is 12% of the mass of the polyester to obtain a mixed raw material.

[0055] S4. Spinning: The dried mixed raw material is dried for a second time, and melt-spinned in a melt spinning machine with a melt temperature of 280° C. and a spinneret diameter of 0.35 mm to form primary fibers.

[0056] S5. Post-treatment: The spun fibers are subjected to multi-stage stretching. During the stretching process, segmented temperature control is adopted. The number of multi-stage stretching is 2, and the stretching multiple of each stage is 2.5. The segmented temperature control is 3 sections, with the first section being 100°C, the second section being 150°C, and the third section being 200°C. Then, heat setting is performed. Microwave-assisted heating is adopted during heat setting. The power of microwave-assisted heating is 1200W, and the heating time is 15min, so that the internal structure of the fiber is more stable, and skin-friendly and antibacterial fibers are obtained.

[0057] The preparation method of the antibacterial compound is as follows:

[0058] (1) 20 g of maleic anhydride was dissolved in 120 mL of anhydrous ethanol to prepare a solution, 16 g of guanidine hydrochloride was added and stirred, nitrogen was passed through for 40 min, and the mixture was stirred in a water bath at 80° C. for 8 h to obtain functionalized maleic anhydride;

[0059] (2) 30 g of functionalized maleic anhydride was dissolved in 150 mL of anhydrous ethanol, 15 g of 2,3-epoxypropyltrimethylammonium chloride was added thereto, the mixture was stirred evenly, 2.4 g of catalyst stannous octoate was added, and the mixture was reacted for 3 h to obtain a reaction solution; 24 g of 2-vinylimidazole was added to 200 mL of anhydrous ethanol, stirred to dissolve, and then mixed with the reaction solution, 3 g of 2% azobisisobutyronitrile was added, and the mixture was reacted in a constant temperature water bath at 100 ° C for 10 h. After the reaction was completed, the mixture was precipitated with distilled water and dried in a vacuum drying oven at 80 ° C for 20 h to obtain an antibacterial compound.

[0060] The preparation method of the antistatic agent is as follows:

[0061] (3) 200 g of chitosan was dissolved in 2000 mL of 10% glacial acetic acid solution to prepare a chitosan solution, and 80 g of acrylamide was dissolved in 800 mL of water to prepare an acrylamide solution. The chitosan was heated to 60° C. and then added to the acrylamide solution. 30 g of initiator ammonium persulfate was added, the temperature was raised to 100° C. and the reaction was carried out for 6 h, and then the grafted product was obtained by drying.

[0062] (4) 20 g of diethylenetriamine was slowly dripped into 30 g of ethyl acrylate and 80 mL of methanol solution under nitrogen protection, reacted for 5 h, and the methanol was removed under reduced pressure. The temperature was raised to 150 ° C. and the reaction was carried out under reduced pressure for 6 h. After the reaction was completed, water was added and stirred evenly. 16 g of 2-epoxypropyl dodecyl dimethyl quaternary ammonium salt was added thereto, and the reaction was stirred at 80 ° C. for 30 min. Acetone was added for precipitation and separation, and vacuum drying was performed to obtain a modified quaternary ammonium salt;

[0063] (5) 20 g of modified quaternary ammonium salt, 100 g of grafted product, 500 mL of anhydrous ethanol, and 6 g of initiator benzoyl peroxide were mixed, stirred and reacted at 80° C. for 10 h, and dried after the reaction to obtain an antistatic agent.

[0064] Example 3

[0065] S1. Pretreatment of waste polyester: sort the waste polyester to remove non-polyester components and polyester materials that are severely damaged or stained with stubborn stains. Then perform deep cleaning, including ultrasonic cleaning and chemical cleaning, to remove fine impurities and residual stains. The cleaning agent used for chemical cleaning is sodium carbonate solution with a mass concentration of 6%. Finally, dry it to ensure that the moisture content of the waste polyester is less than 5%.

[0066] S2. Impurity removal: The pretreated waste polyester is placed in a composite solvent containing dimethylformamide and dimethyl sulfoxide in a mass ratio of 1:1. The mixture is stirred at a stirring speed of 450 r / min for 45 minutes. At the same time, inert gas nitrogen is introduced for protection to prevent oxidation of the solution. High-quality polyester is obtained by filtration.

[0067] S3, additive mixing: the polyester in S2 is dried and crushed, and a skin-friendly agent, an antibacterial compound and an antistatic agent are added thereto. The skin-friendly agent is sodium hyaluronate with a natural moisturizing factor, and the amount of the skin-friendly agent added is 10% of the mass of the polyester to obtain a mixed raw material.

[0068] S4. Spinning: The dried mixed raw materials are secondary dried and melt-spun in a melt spinning machine with a melt temperature of 250° C. and a spinneret hole diameter of 0.2 mm to form primary fibers.

[0069] S5. Post-treatment: The spun fibers are subjected to multi-stage stretching. During the stretching process, segmented temperature control is adopted. The number of multi-stage stretching is 2, and the stretching multiple of each stage is 1.8. The segmented temperature control is 3 sections, with the first section being 80°C, the second section being 120°C, and the third section being 150°C. Then, heat setting is performed. Microwave-assisted heating is adopted during heat setting. The power of microwave-assisted heating is 1000W, and the heating time is 15 minutes, so that the internal structure of the fiber is more stable, and skin-friendly and antibacterial fibers are obtained.

[0070] The preparation method of the antibacterial compound is as follows:

[0071] (1) 20 g of maleic anhydride was dissolved in 120 mL of anhydrous ethanol to prepare a solution, 15 g of guanidine hydrochloride was added and stirred, nitrogen was passed through for 40 min, and the mixture was stirred in a 70° C. water bath for 5 h to obtain functionalized maleic anhydride;

[0072] (2) 30 g of functionalized maleic anhydride was dissolved in 150 mL of anhydrous ethanol, 8 g of 2,3-epoxypropyltrimethylammonium chloride was added thereto, the mixture was stirred evenly, 1.8 g of catalyst stannous octoate was added, and the mixture was reacted for 2 h to obtain a reaction solution; 18 g of 2-vinylimidazole was added to 180 mL of anhydrous ethanol, stirred to dissolve, and then mixed with the reaction solution, 2 g of 2% azobisisobutyronitrile was added, and the mixture was reacted in a constant temperature water bath at 90 ° C for 6 h. After the reaction was completed, the mixture was precipitated with distilled water and dried in a vacuum drying oven at 80 ° C for 15 h to obtain an antibacterial compound.

[0073] The preparation method of the antistatic agent is as follows:

[0074] (3) 120 g of chitosan was dissolved in 1500 mL of 10% glacial acetic acid solution to prepare a chitosan solution, and 62 g of acrylamide was dissolved in 600 mL of water to prepare an acrylamide solution. The chitosan was heated to 60° C. and then added to the acrylamide solution. 15 g of initiator ammonium persulfate was added, the temperature was raised to 90° C. for reaction for 3 h, and then dried to obtain a grafted product.

[0075] (4) 10 g of diethylenetriamine was slowly dripped into 15 g of ethyl acrylate and 60 mL of methanol solution under nitrogen protection, and the reaction was carried out for 3 h. The methanol was removed under reduced pressure, and the temperature was raised to 150° C. and the reaction was carried out under reduced pressure for 3 to 6 h. After the reaction was completed, water was added and stirred evenly. 5 g of 2-epoxypropyl dodecyl dimethyl quaternary ammonium salt was added thereto, and the reaction was stirred at 80° C. for 10 min. Acetone was added for precipitation and separation, and vacuum drying was performed to obtain a modified quaternary ammonium salt;

[0076] (5) 15 g of modified quaternary ammonium salt, 70 g of grafted product, 400 mL of anhydrous ethanol, and 5 g of initiator benzoyl peroxide were mixed, stirred and reacted at 60° C. for 6 h, and dried after the reaction to obtain an antistatic agent.

[0077] Example 4

[0078] S1. Pretreatment of waste polyester: sort the waste polyester to remove non-polyester components and polyester materials that are severely damaged or stained with stubborn stains. Then perform deep cleaning, including ultrasonic cleaning and chemical cleaning, to remove fine impurities and residual stains. The cleaning agent used for chemical cleaning is sodium carbonate solution with a mass concentration of 8%. Finally, dry it to ensure that the moisture content of the waste polyester is less than 5%.

[0079] S2. Impurity removal: The pretreated waste polyester is placed in a composite solvent containing dimethylformamide and dimethyl sulfoxide in a mass ratio of 1:1.2, and stirred continuously for 50 minutes at a stirring speed of 300 r / min. At the same time, inert gas nitrogen is introduced for protection to prevent the solution from oxidation, and high-quality polyester is obtained by filtration.

[0080] S3, additive mixing: the polyester in S2 is dried and crushed, and a skin-friendly agent, an antibacterial compound and an antistatic agent are added thereto. The skin-friendly agent is sodium hyaluronate with a natural moisturizing factor, and the amount of the skin-friendly agent added is 10% of the mass of the polyester to obtain a mixed raw material.

[0081] S4. Spinning: The dried mixed raw materials are dried for a second time and melt-spun in a melt spinning machine with a melt temperature of 260° C. and a spinneret diameter of 0.25 mm to form primary fibers.

[0082] S5. Post-treatment: The spun fibers are subjected to multi-stage stretching. During the stretching process, segmented temperature control is adopted. The number of multi-stage stretching is 2, and the stretching multiple of each stage is 2.5. The segmented temperature control is 3 sections, with the first section being 90°C, the second section being 140°C, and the third section being 190°C. Then, heat setting is performed. Microwave-assisted heating is adopted during heat setting. The power of microwave-assisted heating is 1200W, and the heating time is 10 minutes, so that the internal structure of the fiber is more stable, and skin-friendly and antibacterial fibers are obtained.

[0083] The preparation method of the antibacterial compound is as follows:

[0084] (1) 20 g of maleic anhydride was dissolved in 120 mL of anhydrous ethanol to prepare a solution, 14 g of guanidine hydrochloride was added and stirred, nitrogen was passed through for 30 min, and the mixture was stirred in a 60° C. water bath for 6 h to obtain functionalized maleic anhydride;

[0085] (2) 30 g of functionalized maleic anhydride was dissolved in 150 mL of anhydrous ethanol, 10 g of 2,3-epoxypropyltrimethylammonium chloride was added thereto, the mixture was stirred evenly, 2 g of catalyst stannous octoate was added, and the mixture was reacted for 3 h to obtain a reaction solution; 20 g of 2-vinylimidazole was added to 200 mL of anhydrous ethanol, stirred to dissolve, and then mixed with the reaction solution, 2.5 g of 2% azobisisobutyronitrile was added, and the mixture was reacted in a constant temperature water bath at 80 ° C for 8 h. After the reaction was completed, the mixture was precipitated with distilled water and dried in a vacuum drying oven at 80 ° C for 15 h to obtain an antibacterial compound.

[0086] The preparation method of the antistatic agent is as follows:

[0087] (3) 150 g of chitosan was dissolved in 1800 mL of 10% glacial acetic acid solution to prepare a chitosan solution, and 80 g of acrylamide was dissolved in 800 mL of water to prepare an acrylamide solution. The chitosan was heated to 50° C. and then added to the acrylamide solution. 20 g of initiator ammonium persulfate was added, the temperature was raised to 100° C. and the reaction was carried out for 5 h, and then the grafted product was obtained by drying.

[0088] (4) 20 g of diethylenetriamine was slowly dripped into 30 g of ethyl acrylate and 60 mL of methanol solution under nitrogen protection, reacted for 4 h, and the methanol was removed under reduced pressure. The temperature was raised to 130 ° C. and the reaction was carried out under reduced pressure for 4 h. After the reaction was completed, water was added and stirred evenly. 10 g of 2-epoxypropyl dodecyl dimethyl quaternary ammonium salt was added thereto, and the reaction was stirred at 80 ° C. for 30 min. Acetone was added for precipitation and separation, and vacuum drying was performed to obtain a modified quaternary ammonium salt;

[0089] (5) 20 g of modified quaternary ammonium salt, 100 g of grafted product, 500 mL of anhydrous ethanol, and 3 g of initiator benzoyl peroxide were mixed, stirred and reacted at 80° C. for 10 h, and dried after the reaction to obtain an antistatic agent.

[0090] Example 5

[0091] S1. Pretreatment of waste polyester: sort the waste polyester to remove non-polyester components and polyester materials that are severely damaged or stained with stubborn stains. Then perform deep cleaning, including ultrasonic cleaning and chemical cleaning, to remove fine impurities and residual stains. The cleaning agent used for chemical cleaning is sodium carbonate solution with a mass concentration of 10%. Finally, dry it to ensure that the moisture content of the waste polyester is less than 5%.

[0092] S2. Impurity removal: The pretreated waste polyester is placed in a composite solvent containing dimethylformamide and dimethyl sulfoxide in a mass ratio of 1:0.8, and stirred continuously for 340 minutes at a stirring speed of 400 r / min. At the same time, inert gas nitrogen is introduced for protection to prevent oxidation of the solution, and high-quality polyester is obtained by filtration.

[0093] S3, additive mixing: the polyester in S2 is dried and crushed, and a skin-friendly agent, an antibacterial compound and an antistatic agent are added thereto. The skin-friendly agent is sodium hyaluronate with a natural moisturizing factor, and the amount of the skin-friendly agent added is 8% of the mass of the polyester to obtain a mixed raw material.

[0094] S4. Spinning: The dried mixed raw materials are dried for a second time and melt-spun in a melt spinning machine with a melt temperature of 240° C. and a spinneret hole diameter of 0.3 mm to form primary fibers.

[0095] S5. Post-treatment: The spun fibers are subjected to multi-stage stretching. During the stretching process, segmented temperature control is adopted. The number of multi-stage stretching is 2, and the stretching multiple of each stage is 1.5. The segmented temperature control is 3 sections, with the first section being 80°C, the second section being 150°C, and the third section being 200°C. Then, heat setting is performed. Microwave-assisted heating is adopted during heat setting. The power of microwave-assisted heating is 800W, and the heating time is 15 minutes, so that the internal structure of the fiber is more stable, and skin-friendly and antibacterial fibers are obtained.

[0096] The preparation method of the antibacterial compound is as follows:

[0097] (1) 20 g of maleic anhydride was dissolved in 120 mL of anhydrous ethanol to prepare a solution, 15 g of guanidine hydrochloride was added and stirred, nitrogen was passed for 40 min, and the mixture was stirred in a water bath at 80° C. for 6 h to obtain functionalized maleic anhydride;

[0098] (2) 30 g of functionalized maleic anhydride was dissolved in 150 mL of anhydrous ethanol, 12 g of 2,3-epoxypropyltrimethylammonium chloride was added thereto, the mixture was stirred evenly, 2.4 g of catalyst stannous octoate was added, and the mixture was reacted for 1 h to obtain a reaction solution; 22 g of 2-vinylimidazole was added to 200 mL of anhydrous ethanol, stirred to dissolve, and then mixed with the reaction solution, 3 g of 2% azobisisobutyronitrile was added, and the mixture was reacted in a constant temperature water bath at 80 ° C for 10 h. After the reaction was completed, the mixture was precipitated with distilled water and dried in a vacuum drying oven at 60 ° C for 18 h to obtain an antibacterial compound.

[0099] The preparation method of the antistatic agent is as follows:

[0100] (3) 100 g of chitosan was dissolved in 2000 mL of 10% glacial acetic acid solution to prepare a chitosan solution, and 60 g of acrylamide was dissolved in 500 mL of water to prepare an acrylamide solution. The chitosan was heated to 50° C. and then added to the acrylamide solution. 20 g of initiator ammonium persulfate was added, the temperature was raised to 900° C. for reaction for 6 h, and then dried to obtain a grafted product.

[0101] (4) 15 g of diethylenetriamine was slowly dripped into 20 g of ethyl acrylate and 60 mL of methanol solution under nitrogen protection, and the reaction was carried out for 4 h. Methanol was removed under reduced pressure, and the temperature was raised to 150° C. and the reaction was carried out under reduced pressure for 6 h. After the reaction was completed, water was added and stirred evenly. 16 g of 2-epoxypropyl dodecyl dimethyl quaternary ammonium salt was added thereto, and the reaction was stirred at 80° C. for 10 min. Acetone was added for precipitation and separation, and vacuum drying was performed to obtain a modified quaternary ammonium salt;

[0102] (5) 10 g of modified quaternary ammonium salt, 60 g of grafted product, 200 mL of anhydrous ethanol, and 5 g of initiator benzoyl peroxide were mixed, stirred and reacted at 80° C. for 6 h, and dried after the reaction to obtain an antistatic agent.

[0103] Comparative Example 1: The preparation method is the same as that of Example 1, but no antibacterial compound is added.

[0104] Comparative Example 2: The preparation method is the same as that of Example 1, without adding an antistatic agent, and step S4 is modified as follows: electrospinning is adopted with a voltage of 20 kV and a distance between the nozzle and the receiving device of 15 cm to obtain nascent fibers.

[0105] Comparative Example 3: The preparation method is the same as that of Example 1, and step S5 is modified as follows: pulling, stretching, and shaping the nascent fibers.

[0106] Performance Test:

[0107] 1. Antibacterial performance test: The antibacterial rate was calculated by comparing the colony count of Staphylococcus aureus cultured in agar medium for 24 hours using the oscillation method GB / T 20944.3. The results are shown in Table 1.

[0108] Table 1

[0109] Group Antibacterial rate% Example 1 96.88 Example 2 95.65 Example 3 97.38 Example 4 96.75 Example 5 96.62 Comparative Example 1 66.25

[0110] It can be seen from Table 1 that the antibacterial rates of Examples 1 to 5 are higher, and the skin-friendly antibacterial fibers of Examples 1 to 5 have good antibacterial properties.

[0111] 2. Antistatic performance test: According to GB / T 12703-1991, the half-life method is used to discharge the sample placed on a rotating metal platform with a high voltage of 10KV for 30s. When the static voltage is stable, the time and half-life when the induced voltage decays to half are detected. The results are shown in Table 2.

[0112] Table 2

[0113] Group Half-life / s Example 1 2.35 Example 2 2.28 Example 3 2.36 Example 4 2.56 Example 5 2.54 Comparative Example 2 6.85

[0114] It can be seen from Table 2 that the skin-friendly antibacterial fibers of Examples 1 to 5 have good antistatic properties.

[0115] 3. Breaking strength test:

[0116] Group Fiber fineness dtex Breaking strength cN / dtex Example 1 1.0 4.2 Example 2 1.0 4.3 Example 3 1.0 4.0 Example 4 1.0 4.2 Example 5 1.0 4.2 Comparative Example 3 1.0 2.8

[0117] It can be seen from Table 3 that the breaking strength of Examples 1 to 5 is greater, and the strength of the skin-friendly antibacterial fiber is higher.

[0118] It can be seen from the above table that the skin-friendly antibacterial fibers prepared in Examples 1 to 5 of the present invention have good antibacterial properties, antistatic properties and high strength. The skin-friendly antibacterial fibers are made into clothing, and after skin moisture testing, the skin moisture content increase rate reaches more than 20%.

[0119] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

[0120] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for recycling waste polyester to prepare skin-friendly antibacterial fibers, Features: The following steps are involved: S1. Pretreatment of waste polyester: sort the waste polyester to remove non-polyester components and polyester materials that are severely damaged or stained with stubborn stains, then perform deep cleaning and finally dry to ensure that the moisture content of the waste polyester is less than 5%; S2, impurity removal: the pretreated waste polyester is placed in a composite solvent, stirred continuously for 30 to 60 minutes at a stirring speed of 300 to 500 r / min, and inert gas nitrogen is introduced to protect the solution to prevent oxidation, and high-quality polyester is obtained by filtering; S3, additive mixing: drying and crushing the polyester in S2, adding a skin-friendly agent, an antibacterial compound and an antistatic agent thereto to obtain a mixed raw material; S4, spinning: the dried mixed raw material is subjected to secondary drying, and melt-spinning is performed in a melt spinning machine to form primary fibers; S5. Post-treatment: The nascent fiber is subjected to multi-stage stretching, and segmented temperature control is adopted during the stretching process, and then heat setting is performed. Microwave-assisted heating is adopted during heat setting. The power of microwave-assisted heating is 800-1200W, and the heating time is 10-15min, so that the internal structure of the fiber is more stable, and skin-friendly and antibacterial fiber is obtained.

2. The method for preparing skin-friendly and antibacterial fiber by recycling and regenerating waste polyester according to claim 1, Features: The deep cleaning in step S1 includes ultrasonic cleaning and chemical cleaning. The cleaning agent used in the chemical cleaning is a sodium carbonate solution with a mass concentration of 5-10%.

3. The method for preparing skin-friendly and antibacterial fiber by recycling and regenerating waste polyester according to claim 1, Features: In step S2, the composite solvent is dimethylformamide and dimethyl sulfoxide in a mass ratio of 1:0.8-1.

2.

4. The method for preparing skin-friendly and antibacterial fiber by recycling and regenerating waste polyester according to claim 1, Features: In step S3, the skin-friendly agent is sodium hyaluronate having a natural moisturizing factor, and the amount of the skin-friendly agent added is 8-12% of the mass of the polyester.

5. The method for preparing skin-friendly and antibacterial fiber by recycling and regenerating waste polyester according to claim 1, Features: The melt temperature of the melt spinning process in step S4 is 230-280° C., and the diameter of the spinneret hole is 0.15-0.35 mm.

6. The method for preparing skin-friendly and antibacterial fiber by recycling and regenerating waste polyester according to claim 1, Features: The number of multi-stage stretching in step S5 is 2, and the stretching multiple of each stage is 1.2-2.5; the segmented temperature control is 3 stages, stage 1 is 70-100°C, stage 2 is 110-150°C, and stage 3 is 140-200°C.

7. The method for preparing skin-friendly and antibacterial fibers by recycling and regenerating waste polyester according to claim 1, Features: The preparation method of the antibacterial compound and the antistatic agent in step (1) is as follows: (1) dissolving maleic anhydride in anhydrous ethanol to prepare a solution, adding guanidine hydrochloride and stirring, passing nitrogen for 30 to 40 minutes, stirring and reacting in a water bath at 60 to 80° C. for 3 to 8 hours to obtain functionalized maleic anhydride; (2) dissolving functionalized maleic anhydride in anhydrous ethanol, adding 2,3-epoxypropyltrimethylammonium chloride thereto, stirring evenly, adding a catalyst stannous octoate, reacting for 1 to 3 hours, and obtaining a reaction solution; adding 2-vinylimidazole to anhydrous ethanol, stirring to dissolve, and then mixing with the reaction solution, adding 2% by mass of azobisisobutyronitrile, and reacting in a constant temperature water bath at 80 to 100° C. for 5 to 10 hours, and after the reaction is completed, precipitating with distilled water, and drying in a vacuum drying oven at 60 to 80° C. for 10 to 20 hours to obtain an antibacterial compound; (3) dissolving chitosan in a 10% by mass glacial acetic acid solution to prepare a chitosan solution, then dissolving acrylamide in water to prepare an acrylamide solution, heating the chitosan to 50-60° C. and adding it to the acrylamide solution, adding an initiator, ammonium persulfate, heating to 80-100° C. to react for 2-6 hours, and drying to obtain a grafted product; (4) slowly dripping diethylenetriamine into the ethyl acrylate and methanol solution under nitrogen protection, reacting for 2 to 5 hours, removing methanol under reduced pressure, heating to 120 to 150° C. and reacting under reduced pressure for 3 to 6 hours, adding water and stirring evenly after the reaction, adding 2-epoxypropyl dodecyl dimethyl quaternary ammonium salt, stirring and reacting at 60 to 80° C. for 10 to 30 minutes, adding acetone for precipitation and separation, and vacuum drying to obtain a modified quaternary ammonium salt; (5) The modified quaternary ammonium salt, the grafted product, anhydrous ethanol, and the initiator benzoyl peroxide are mixed, stirred and reacted at 60 to 80° C. for 6 to 10 hours, and dried after the reaction to obtain an antistatic agent.

8. The method for preparing skin-friendly and antibacterial fibers by recycling and regenerating waste polyester according to claim 7, Features: In the step (1), the mass ratio of maleic anhydride to guanidine hydrochloride is 1:0.6-0.8; in the step (2), the mass ratio of functionalized maleic anhydride, 2,3-epoxypropyltrimethylammonium chloride, stannous octoate, 2-vinylimidazole, and 2% azobisisobutyronitrile is 1:0.2-0.5:0.05-0.08:0.5-0.8:0.05-0.

1.

9. The method for preparing skin-friendly and antibacterial fiber by recycling and regenerating waste polyester according to claim 7, Features: In the step (3), the mass ratio of chitosan, acrylamide and initiator ammonium persulfate is 1:0.6-0.8:0.1-0.3; in the step (4), the mass ratio of diethylenetriamine, ethyl acrylate and 2-epoxypropyl dodecyl dimethyl quaternary ammonium salt is 1:1.2-1.5:0.4-0.8; in the step (5), the mass ratio of modified quaternary ammonium salt, grafted product and initiator benzoyl peroxide is 1:5-7:0.1-0.

3.

10. The skin-friendly antibacterial fiber prepared by the method for preparing skin-friendly antibacterial fiber by recycling waste polyester according to claim 1, Features: The skin-friendly antibacterial fiber is used in the fields of automobile apparel, home textiles, clothing, and building materials.