Oil stain easy-to-clean down jacket fabric and preparation method thereof

By filling the down jacket fabric with nanographene and calcium hydrogenphosphite particles and using snail extract to treat nylon fiber, the problem of oil stains being difficult to clean when cleaning the down jacket fabric is improved, and the anti-fouling and easy decontamination are enhanced. Antioxidant and antistatic properties are reduced, friction and fiber pilling are improved, and the overall performance of the fabric is improved.

CN118932704AInactive Publication Date: 2024-11-12GAOFAN (ZHEJIANG) INFORMATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411025727.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When using and cleaning, existing down jacket fabrics are easily damaged due to fiber wrapping, oil stains are difficult to clean, and wear resistance leads to increased friction, affecting cleaning convenience.

Method used

Using the treated nylon fibers to heat textiles, fill nanographene particles and calcium hydrogenphosphite particles, and use snail extract as a loading liquid, and finish them by ultrasonic treatment and decontamination finishing agent to prepare anti-fouling composite fabrics to improve stain resistance. And easy to decontaminate.

Benefits of technology

It effectively increases the anti-fouling properties of the fabric, prevents oil stains, improves cleaning efficiency, reduces friction and fiber pilling, enhances anti-oxidation and anti-static properties, and maintains the brightness and moisturizing properties of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968473470000061
    Figure BDA0004968473470000061
  • Figure BDA0004968473470000071
    Figure BDA0004968473470000071
  • Figure BDA0004968473470000081
    Figure BDA0004968473470000081
Patent Text Reader

Abstract

The invention discloses an oil stain easy-to-clean down jacket fabric and a preparation method, and relates to the field of down jacket fabrics, and the oil stain easy-to-clean down jacket fabric is obtained by finishing an antifouling compound fabric with a decontamination finishing agent. The antifouling composite fabric is obtained by spinning treated polyamide fibers under the heating condition, the treated polyamide fibers are prepared from polyamide fibers and filling particles loaded in gaps in the surfaces of the polyamide fibers, and the filling particles comprise nano graphene particles and calcium hydrogen phosphate particles. The calcium hydrogen phosphate particles and the nano graphene particles are adopted as filling particles of the chinlon fabric, the antifouling property of the fabric is effectively improved, oil stains are prevented from coloring the fabric, and the calcium hydrogen phosphate particles can accelerate combination of oil drops and a detergent during cleaning, so that the effect of rapid decontamination is achieved; and calcium hydrogen phosphite has excellent oxidation resistance and salt resistance, and can protect the fabric in the washing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of down jacket fabrics, and particularly relates to an oil stain-easy-to-clean down jacket fabric and a preparation method thereof. Background Art

[0002] Down jackets are often worn for a long time in winter, so they are often faced with the problem of difficult cleaning of oil stains. The outer fabrics of existing down jackets are mostly nylon fabrics, which have high wear resistance, good elasticity, are not easy to deform, and can maintain warmth in a humid environment. In order to meet the general consumer's needs for cleaning and maintenance of nylon fabrics, the prior art uses a decontamination finishing agent to give nylon fabrics decontamination and easy-to-clean functions. The protective film formed by the decontamination finishing agent and the surface of the nylon fabric exhibits good waterproof and oil-proof properties, which can effectively prevent the invasion and deposition of water and oil droplets, making the cleaning of nylon fabrics more convenient and efficient.

[0003] However, due to the high wear resistance of nylon fabric, the most frequently used parts such as collars, cuffs, front lapels, hems, and pockets will rub against each other during use and cleaning, and the fibers will become entangled into a ball shape, destroying the protective film on the surface of the fabric, causing the down jacket fabric to lose its anti-fouling ability, and oil stains can easily enter the interior of the fibers, making them difficult to clean. Summary of the invention

[0004] The purpose of the present invention is to provide a down jacket fabric that is easy to clean from oil stains and a preparation method in order to solve the above problems.

[0005] The present invention achieves the above-mentioned purpose through the following synthesis process and technical scheme:

[0006] The present invention provides a down jacket fabric that is easy to clean from oil stains. The down jacket fabric that is easy to clean from oil stains is obtained by finishing an anti-fouling composite fabric with a decontamination finishing agent.

[0007] The antifouling composite fabric is obtained by weaving treated nylon fibers under heating conditions. The treated nylon fibers are made of nylon fibers and filling particles loaded in the gaps on the surfaces of the nylon fibers. The filling particles include nanographene particles and calcium hydrogen phosphite particles, and the calcium hydrogen phosphite particles account for 35-45% of the total mass percentage of the filling particles.

[0008] As a further optimization scheme of the present invention, the preparation method of the treated nylon fiber comprises the following steps:

[0009] (1) subjecting nylon polymer to a stretching and heat setting process in sequence to obtain nylon fiber;

[0010] (2) Immersing the nylon fiber in a loading liquid containing the filling particles for ultrasonic treatment, and then drying to obtain the treated nylon fiber, wherein the loading liquid is composed of 75wt% ethanol and snail extract in a volume ratio of 1:(0.1-0.2).

[0011] As a further optimization scheme of the present invention, step (1) is specifically as follows: the nylon polymer is carded and then put into a drawing machine for stretching, and after stretching, it is placed in a polyvinyl pyrrolidone solution for immersion treatment to obtain pre-impregnated nylon fiber, and then placed in a setting machine for high-temperature setting, and the fiber is obtained after setting and drying;

[0012] Among them, the stretching speed is 2-5m / min and the setting temperature is 160-180℃.

[0013] As a further optimization scheme of the present invention, the preparation process of the snail extract is specifically as follows: the shelled tissue of the cultured snail is put into boiling water and boiled, a preservative is added during the boiling process, and after boiling into a thick soup, the tissue is put into a grid mold and frozen into a solid, and the solid is demolded and placed in a vacuum dryer for drying, and then ground with a grinder to obtain the snail extract.

[0014] As a further optimization scheme of the present invention, the preservative is one of sorbic acid and its salts, benzoic acid and its sodium salt.

[0015] As a further optimization scheme of the present invention, the ultrasonic treatment time is 15-20 minutes, the ultrasonic power is 100-300W, and the ultrasonic frequency is 20-30KHz.

[0016] As a further optimization solution of the present invention, the fineness of the nylon fiber is 15-20D.

[0017] As a further optimization scheme of the present invention, the preparation process of the calcium hydrogen phosphite particles is specifically as follows: phosphorous acid, aluminum oxide, boric acid, calcium chloride and ammonia water are added to a reactor, the reactor is placed in a hydrothermal reactor, and the reaction is carried out for 50-60 hours. After the reaction is completed, it is naturally cooled to room temperature, the solid phase mixture in the reactor is repeatedly washed with boiling water and dried, and finally the calcium hydrogen phosphite particles are obtained after grinding with a nano-scale grinder.

[0018] The present invention also provides a method for preparing the above fabric, comprising the following steps:

[0019] (1) preparing treated nylon fibers, warping the treated nylon fibers and weaving them on a machine, heating the textile rollers during weaving, and cooling and winding the treated nylon fibers after weaving to obtain an antifouling composite fabric;

[0020] (2) The anti-fouling composite fabric is treated in an aqueous solution of a soil-removing finishing agent to obtain the fabric, wherein the soil-removing finishing agent is a triple-proof easy-to-remove finishing agent.

[0021] As a further optimization scheme of the present invention, the heating temperature is 160-180°C.

[0022] The beneficial effects of the present invention are:

[0023] The present invention adopts calcium hydrogen phosphite particles and nanographene particles as filling particles of nylon fabric, which can effectively increase the antifouling property of fabric, prevent oil stains from being colored on fabric, and accelerate the combination of oil droplets and detergents during cleaning through calcium hydrogen phosphite particles, so that it can achieve the effect of rapid decontamination, and calcium hydrogen phosphite has excellent antioxidant properties and salt resistance, and can protect fabrics in the washing process, and through nanographene particles, which have heat preservation and antibacterial properties, and have excellent antistatic properties and certain lubrication properties, the friction factor of fabrics can be reduced, and the loss of calcium hydrogen phosphite particles during washing can be reduced. Further, in the process of treating nylon fiber, snail extract is used as a component of the loading liquid, and the filling particles are loaded into the nylon fiber. The viscosity of the snail extract is used to increase the force between fibers, prevent pilling, and have stronger adhesion and better stability, and can prevent oil stains from being colored on fabrics, thereby increasing the brightness of fabrics. DETAILED DESCRIPTION

[0024] The present application is described in further detail below. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technicians in this field can make some non-essential improvements and adjustments to the present application based on the above application content.

[0025] 1. Materials

[0026] (1) Nanographene particles were purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0027] (2) The nylon polymer was PA6 fiber purchased from Ningbo Shijin Plastic Co., Ltd.

[0028] (3) The snail extract preparation process is as follows: farmed snails (purchased from Jiaxing Hongfu Snail Farming Co., Ltd.) are washed with a mixture of edible oil and water to completely remove impurities, then shelled by machine, and the snail tissue after shelling is put into boiling water at 100°C and boiled until the boiling water covers the snail tissue. During the boiling process, a preservative potassium sorbate or sodium benzoate (potassium sorbate is used in this embodiment) is added. After boiling until a thick soup is formed, the snail is put into a grid mold and frozen in a freezer at -80--50°C to form a solid naturally. After the solid is demolded, it is put into a vacuum dryer for drying at a vacuum degree of 0.1-0.5 mbar for 24-48 hours, and then ground by a grinder to obtain the snail extract.

[0029] (4) The preparation process of calcium hydrogen phosphite particles is specifically as follows: phosphorous acid H3PO3, aluminum oxide Al2O3, boric acid H3BO3, calcium chloride CaCl2 and ammonia water NH3(H2O) (stoichiometric ratio is 0.15:0.05:1:0.25:1) are added to the lining of a reactor, the lining of the reactor is placed in a hydrothermal reactor, and the reaction is carried out for 50-60 hours at a heating temperature of 200-300°C (the temperature range used in this embodiment is 220-250°C). After the reaction is completed, the mixture is naturally cooled to room temperature, the solid phase mixture in the reactor is repeatedly washed with boiling water and dried, and finally ground by a nano-grinding machine to obtain calcium hydrogen phosphite particles with a particle size of ≤20μm.

[0030] (5) Three-proof and easy-to-remove finishing agent, purchased from Shanghai Green Copper Materials Co., Ltd.

[0031] The methods used in this example are conventional methods known to those skilled in the art unless otherwise specified, and the reagents and other materials used are commercially available products unless otherwise specified.

[0032] 2. Example

[0033] Example 1

[0034] The oil stain easy-to-clean down jacket fabric of this embodiment is prepared as follows:

[0035] (1) Preparation and treatment of nylon fiber

[0036] The nylon polymer is sequentially subjected to a stretching and heat setting process to obtain nylon fiber; specifically:

[0037] First, the nylon polymer (PA6 fiber) is carded and then put into a drawing machine for stretching at a stretching speed of 4m / min. After stretching, it is immersed in a polyvinyl pyrrolidone solution (15% w / v) to obtain pre-impregnated nylon fiber, and then placed in a setting machine for high-temperature setting at a setting temperature of 180°C. After setting and drying, the nylon fiber is obtained, wherein the fineness of the nylon fiber is controlled within the range of 15-20D by controlling the parameters of the drawing machine and the setting machine;

[0038] The nylon fiber is immersed in a loading liquid containing filling particles for ultrasonic treatment, the ultrasonic treatment time is 20 minutes, the ultrasonic power is 100W, the ultrasonic frequency is 20KHz, and then dried to obtain the treated nylon fiber, wherein the calcium hydrogen phosphite particles account for 30% of the total mass of the filling particles, and the rest are nanographene particles, and the loading liquid is composed of 75wt% ethanol and snail extract in a volume ratio of 1:0.1.

[0039] (2) The treated nylon fibers are warped and woven on a machine with warp density of 950 strands / 10 cm and weft density of 950 strands / 10 cm. During weaving, the textile roller is heated to 160° C. to promote the bonding of the load liquid to the fibers. After weaving, the woven fabric is cooled and rolled up to obtain an antifouling composite fabric.

[0040] (3) The antifouling composite fabric is treated in an aqueous solution of a decontamination finishing agent for 2 hours to obtain fabric A, wherein the decontamination finishing agent is a triple-proof easy-to-decontaminate finishing agent, and the amount of the decontamination finishing agent used is 50 g / L.

[0041] The preparation process of fabric BG is the same as that of fabric A, the only difference is the change in the mass of calcium hydrogen phosphite particles to the total mass of the filling particles, as shown in Table 1 below:

[0042] Table 1 Composition of filling particles in Example 1 (by mass percentage)

[0043]

[0044] Example 2

[0045] The oil stain easy-to-clean down jacket fabric of this embodiment is prepared as follows:

[0046] (2) Preparation and treatment of nylon fiber

[0047] The nylon polymer is sequentially subjected to a stretching and heat setting process to obtain nylon fiber; specifically:

[0048] First, the nylon polymer (PA6 fiber) is carded and then put into a drawing machine for stretching at a stretching speed of 4m / min. After stretching, it is immersed in a polyvinyl pyrrolidone solution (15% w / v) to obtain pre-impregnated nylon fiber, and then placed in a setting machine for high-temperature setting at a setting temperature of 170°C. After setting and drying, the nylon fiber is obtained, wherein the fineness of the nylon fiber is controlled within the range of 15-20D by controlling the parameters of the drawing machine and the setting machine;

[0049] The nylon fiber is immersed in a loading liquid containing filling particles for ultrasonic treatment, the ultrasonic treatment time is 15 minutes, the ultrasonic power is 150W, the ultrasonic frequency is 25KHz, and then dried to obtain the treated nylon fiber, wherein the calcium hydrogen phosphite particles account for 35% of the total mass of the filling particles, and the rest are nanographene particles, and the loading liquid is composed of 75wt% ethanol and snail extract in a volume ratio of 1:0.2.

[0050] (2) The treated nylon fibers were warped and woven on a machine with warp density of 950 strands / 10 cm and weft density of 950 strands / 10 cm. During weaving, the textile rollers were heated to 170° C. After weaving, the woven fabric was cooled and rolled up to obtain a stain-resistant composite fabric.

[0051] (3) The antifouling composite fabric is treated in an aqueous solution of a decontamination finishing agent for 2 hours to obtain fabric H, wherein the decontamination finishing agent is a triple-proof easy-to-decontaminate finishing agent, and the amount of the decontamination finishing agent used is 50 g / L.

[0052] The preparation process of fabric IJ is the same as that of fabric H, except that the composition of the loading liquid is different, as shown in Table 2 below:

[0053] Table 2 Composition of the load solution in Example 2 (v / v)

[0054]

[0055]

[0056] 3. Performance testing

[0057] Take the fabrics prepared in Example 1-2, and set up a blank group and a control group:

[0058] Blank group: 1 is a fabric obtained by spinning and weaving nylon polymer, 2 is a fabric obtained by spinning and weaving nylon fiber in Example 1;

[0059] Control group: 1 is the antifouling composite fabric in the preparation process of fabric B in Example 1, 2 is the fabric obtained by treating the fabric of blank group 1 with an aqueous solution of a decontamination finishing agent for 2 hours, and 3 is the fabric obtained by treating the fabric of blank group 2 with an aqueous solution of a decontamination finishing agent for 2 hours. The decontamination finishing agent is a three-proof easy decontamination finishing agent, and the amount of the decontamination finishing agent used is 50 g / L.

[0060] Take the above fabrics or textiles as samples and perform the following performance tests on them:

[0061] (1) Antifouling performance

[0062] A 30 cm × 12 cm specimen was cut from the non-edge position of each sample, and the specimen was tested by the liquid stain method with reference to GB / T30159.1-2013 “Testing and Evaluation of Antifouling Performance of Textiles Part 1: Stain Resistance”. The specific process is as follows: 2 layers of filter paper are placed on a smooth horizontal surface, and the specimen is placed flatly on the filter paper with the front side facing up. About 0.05 mL of soy sauce liquid is dripped on each of the three parts of the specimen with a dropper, with a spacing of at least 50 mm between each drop. When dripping, the dropper mouth is about 6 mm away from the surface of the specimen. After the specimen has been allowed to stand for 30 seconds, each drop is observed at a viewing angle of about 45° for rating. The rating standards are shown in Table 3 below, and the rating results are statistically obtained in Table 4 below.

[0063] Table 3 Contamination level

[0064]

[0065]

[0066] (2) Easy to clean

[0067] The samples were tested according to the washing method in FZ / T 01118-2012 “Testing and evaluating the antifouling properties of textiles and their stain removal properties”.

[0068] Select peanut oil, take two samples for each sample, drop 0.2mL of dirt on three parts of each sample, cover the dirt with a film, press the hammer for 60 seconds and then leave for 20 minutes, evaluate the initial color difference, wash according to the 6A procedure specified in GB / T8629-2001, spread flat and dry after washing, and use a gray card to evaluate the color difference between the unstained and stained parts of each washed sample. The higher the grade, the better the decontamination performance, and the rating results are shown in Table 5.

[0069] (3) Pilling test

[0070] The pilling test was carried out in accordance with GB / T4802.3-2008 “Test method for fabric pilling—Pilling box method”.

[0071] At room temperature, each sample was washed with clean water in a washing machine for 50 minutes, and then ground 5000 times on a YG(B)511-II rolling box pilling tester. The ground samples were compared with the standard samples to determine the pilling degree of the samples. The pilling degree is divided into five levels (1-5). The smaller the level, the more serious the fabric pilling, and the larger the level, the better the anti-pilling performance. The pilling degree results are statistically obtained in Table 6 below.

[0072] (4) Moisture retention test

[0073] Each sample was cut into 1m×1m size, and the fabric samples were placed in glass dishes and added with the same saturated amount of water, and then placed in a room with the same temperature (20°C) and humidity (40%), and blow-dried with a hair dryer of the same power at a distance of at least 1m. During the drying process, a hygrometer was used to measure the humidity, and the average of 5 groups of experimental data was used as the final data for each group of samples. The following Table 7 was obtained by statistics.

[0074] 4. Results Analysis

[0075] (1) Antifouling performance test results

[0076] Table 4 Contamination level results of each sample

[0077]

[0078] During the test, the surfaces of blank group 1 and blank group 2 were all wetted when droplets were dropped on them. However, it can be clearly found that the wetting speed of blank group 1 is slower than that of blank group 2. The reason is presumably that the antifouling performance of nylon will decrease after the initial nylon polymer is stretched and heat-set, which may be due to the increase in the pores of the nylon polymer itself after the stretching and heat-setting process.

[0079] Comparing the test results of blank group 1-2 and control group 1-3, it is found that the antifouling performance of the fabric obtained by treating nylon fiber is much better than that of nylon polymer. After the nylon polymer is stretched and heat-set and then treated with a decontamination finishing agent, the antifouling effect is improved, but there is still a gap with control group 2-3. The antifouling effect of the nylon polymer fabric that has not been treated in any way after being treated with a decontamination finishing agent is not as good as the fabric obtained by treating nylon fiber alone. By comparing the test results of control group 1 and embodiment 1B, when the droplets are dropped on the fabric sample of embodiment 1B, the droplets are clear and the contact surface of the droplets with the sample is not wetted. When the droplets are dropped on the fabric sample of control group 1, the droplets are partially dark, and more than three-quarters of the liquid volume is retained. It can be seen that the effect of treating nylon fiber on improving the antifouling performance is greater than that of using a decontamination finishing agent;

[0080] The results of Example 1 and Example 2 show that the composition of the filling particles and the loading liquid does not have a significant effect on the antifouling performance of the fabric.

[0081] (2) Test results of easy decontamination performance

[0082] Table 5 Decontamination level of each sample

[0083]

[0084]

[0085] By comparing the results of the easy-to-clean grades of the control groups 1-3, it can be found that the easy-to-clean grade of the anti-fouling composite fabric is better than that of the nylon fabric finished with a decontamination finishing agent. The presumed reason is that filler particles are added to the anti-fouling composite fabric, and the filling particles contain calcium hydrogen phosphite particles. When the fabric is washed in the 6A program, the combination of oil droplets and detergent can be accelerated to achieve a rapid decontamination effect. In addition, calcium hydrogen phosphite has excellent antioxidant properties and salt resistance, which can protect the fabric during the washing program. The filling particles also contain nano-graphene particles, which themselves have heat preservation and antibacterial properties, and have excellent antistatic properties and certain lubricating properties, which can reduce the friction factor of the fabric and reduce the loss of calcium hydrogen phosphite particles during washing.

[0086] By comparing the stain removal levels of various fabrics in Example 1, it was found that when the amount of calcium hydrogen phosphite particles used was greater than 45%, the stain removal effect decreased. The possible reason is that the excessive amount of calcium hydrogen phosphite particles used affected the dispersibility of the filling particles, resulting in a smaller load on the nylon fiber.

[0087] (3) Pilling performance test results

[0088] Table 6 Anti-pilling performance level of each sample

[0089]

[0090]

[0091] By comparing the anti-pilling grade results of control groups 1-3, it can be found that the anti-pilling grade of the anti-fouling composite fabric is significantly better than that of the nylon fabric finished with a decontamination finishing agent. It can be seen from the anti-pilling grades of each sample in Examples 1-2 that the composition change of the filling particles has almost no effect on the anti-pilling performance of the fabric, but the loading liquid used during filling has a greater impact on the anti-pilling performance of the fabric. After the fabric of Example 2J is ground by a rolling box pilling instrument, the surface fibers are filamented into balls, which destroys the barrier of the fabric, so that the fabric is easily contaminated with oil stains. In the process of treating nylon fiber, snail extract is used as a component of the loading liquid, and the filling particles are loaded into the nylon fiber, which has stronger adhesion and better stability, and can prevent oil stains from being colored on the fabric, increasing the brightness of the fabric. More importantly, the snail extract has a certain viscosity. After wrapping the filling particles and loading them on the nylon fiber, it can increase the force between the fibers, prevent pilling, and increase the adhesion with the decontamination finishing agent, so that the overall performance of the fabric remains stable.

[0092] (4) Moisture retention test results

[0093] Table 7 Moisture retention data of each sample

[0094]

[0095]

[0096] It can be seen from the moisturizing test results that the water content of each sample decreases with time. The moisturizing results of the control groups 1-3 and the blank groups 1-2 show that the nylon fabric and the finishing with the decontamination finishing agent have almost no effect on the moisturizing of the fabric. However, the moisturizing results of the control group 1 and the embodiment show that the use of snail extract as a component of the loading liquid can effectively increase the moisturizing performance of the fabric. On the one hand, it is not easy to get oil stains, and on the other hand, it is easy to clean the fabric and make the fabric more comfortable to wear. In addition, the humidity of the control group 1 is reduced to the same as the ambient humidity after 30 minutes, which is much lower than the humidity of the fabric samples in Examples 1 and 2. This shows that although the decontamination finishing agent itself cannot improve the moisturizing performance of the fabric, it has a certain protective effect on the fabric.

[0097] In summary, the present invention uses calcium hydrogen phosphite particles and nanographene particles as filling particles of nylon fabric, which can effectively increase the antifouling property of fabric, prevent oil stains from being colored on fabric, and can accelerate the combination of oil droplets and detergents during cleaning through calcium hydrogen phosphite particles, so that it can achieve the effect of rapid decontamination, and calcium hydrogen phosphite has excellent antioxidant properties and salt resistance, and can protect fabrics in the washing process, through nanographene particles, which itself has heat preservation and antibacterial properties, and has excellent antistatic properties and certain lubrication properties, which can reduce the friction factor of fabrics and reduce the loss of calcium hydrogen phosphite particles during washing. Further, in the process of treating nylon fiber, snail extract is used as a component of the loading liquid, and the filling particles are loaded into nylon fiber. The viscosity of snail extract can be used to increase the force between fibers, prevent pilling, and have stronger adhesion and better stability, and can prevent oil stains from being colored on fabrics, increasing the brightness of fabrics. Adopting the above means, the fabric of the present invention has the effect of anti-oil stains and easy cleaning of oil stains.

[0098] The above-mentioned embodiment only expresses one implementation mode of the present invention, and its description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A down jacket fabric that is easy to clean from oil stains, characterized in that: The oil stain easy-to-clean down jacket fabric is obtained by finishing the anti-fouling composite fabric with a decontamination finishing agent; The antifouling composite fabric is obtained by weaving treated nylon fibers under heating conditions. The treated nylon fibers are made of nylon fibers and filling particles loaded in the gaps on the surfaces of the nylon fibers. The filling particles include nanographene particles and calcium hydrogen phosphite particles.

2. The oil stain easy-to-clean down jacket fabric according to claim 1, characterized in that: The method for preparing the treated nylon fiber comprises the following steps: (1) subjecting nylon polymer to a stretching and heat setting process in sequence to obtain nylon fiber; (2) Immersing the nylon fiber in a loading liquid containing the filling particles for ultrasonic treatment, and then drying to obtain the treated nylon fiber, wherein the loading liquid is composed of 75wt% ethanol and snail extract in a volume ratio of 1:(0.1-0.2).

3. The oil stain easy-to-clean down jacket fabric according to claim 2, characterized in that: Step (1) specifically comprises: the nylon polymer is carded and then put into a drawing machine for stretching, and after the stretching, it is immersed in a polyvinyl pyrrolidone solution to obtain pre-impregnated nylon fiber, and then placed in a setting machine for high-temperature setting, and the fiber is obtained after setting and drying; Among them, the stretching speed is 2-5m / min and the setting temperature is 160-180℃.

4. The oil stain easy-to-clean down jacket fabric according to claim 2, characterized in that: The preparation process of the snail extract is specifically as follows: The shelled tissue of the cultured snail is put into boiling water and boiled, and a preservative is added during the boiling process. After boiling into a thick soup, the tissue is put into a grid mold and frozen into a solid. After the solid is demolded, it is put into a vacuum dryer for drying, and then ground with a grinder to obtain a snail extract.

5. The oil stain easy-to-clean down jacket fabric according to claim 4, characterized in that: The preservative is one of sorbic acid and its salts, benzoic acid and its sodium salt.

6. The oil stain easy-to-clean down jacket fabric according to claim 2, characterized in that: The ultrasonic treatment time is 15-20 minutes, the ultrasonic power is 100-300W, and the ultrasonic frequency is 20-30KHz.

7. The oil stain easy-to-clean down jacket fabric according to claim 1, characterized in that: The fineness of the nylon fiber is 15-20D.

8. The oil stain easy-to-clean down jacket fabric according to claim 1, characterized in that: The calcium hydrogen phosphite particles account for 35-45% of the total mass of the filling particles. The preparation process of the calcium hydrogen phosphite particles is specifically as follows: phosphorous acid, aluminum oxide, boric acid, calcium chloride and ammonia water are added into a reactor, the reactor is placed in a hydrothermal reactor, and the reaction is carried out for 50-60 hours. After the reaction is completed, the reaction is naturally cooled to room temperature, the solid phase mixture in the reactor is repeatedly washed with boiling water and dried, and finally the calcium hydrogen phosphite particles are obtained after grinding with a nano-scale grinder.

9. A method for preparing the oil stain easy-to-clean down jacket fabric according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) preparing treated nylon fibers, warping the treated nylon fibers and weaving them on a machine, heating the textile rollers during weaving, and cooling and winding the treated nylon fibers after weaving to obtain an antifouling composite fabric; (2) The anti-fouling composite fabric is treated in an aqueous solution of a soil-removing finishing agent to obtain the fabric, wherein the soil-removing finishing agent is a triple-proof easy-to-remove finishing agent.

10. The method for preparing the oil stain easy-to-clean down jacket fabric according to claim 9, characterized in that: The heating temperature in step (1) is 160-180°C.