Down feather based on phase change heat storage and temperature regulation, preparation method and application

By embedding a combination of phase-change microcapsules and graphene oxide in the down, using its absorption and release of heat and the moisture-absorbing and expansion characteristics of the concave and convex rod soil, the problem of difficulty in adjusting the temperature by traditional down is solved, and the self-regulating and insulation of down is achieved Performance improvement.

CN118932732APending Publication Date: 2024-11-12ANHUI HUAYING XINTANG DOWN CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192924.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional down is difficult to adjust the temperature by itself in terms of insulation comfort, and the processing process cannot effectively utilize its fluff characteristics to give the self-control function.

Method used

Using a phase change material composed of phase change microcapsules, concave and concave rod soil and graphene oxide, the phase change microcapsules absorb and release heat to adjust the temperature by adjusting the moisture-absorbing and expansion characteristics of concave rod soil. Change materials to reduce the risk of static electricity generation and shedding.

Benefits of technology

The down self-control function is realized, the insulation performance is improved, and the phase change material is maintained during humid environments or during washing, ensuring the fluffyness and insulation performance of the down.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015575900000101
    Figure BDA0005015575900000101
Patent Text Reader

Abstract

The invention discloses down feather based on phase change heat storage and temperature regulation, a preparation method and application, and relates to the technical field of textiles. A phase change material is attached to the surface of the down feather and / or adsorbed in holes; all / part of the phase-change material is embedded into micropores of the down feather; the phase change material is prepared from the following components: 40-60 wt% of a phase change microcapsule; 35 to 45 weight percent of attapulgite; and 5-15 wt% of graphene oxide. The preparation method of the down feather comprises the following steps: mixing attapulgite and graphene oxide to obtain a mixture; mixing the mixture with a phase change microcapsule to obtain a phase change material; and mixing the phase-change material with the down feather, so that the phase-change material is completely / partially embedded into the micropores of the down feather. The down feather is applied to the field of textiles. The phase-change material composed of the phase-change microcapsules, the attapulgite and the graphene oxide is completely / partially embedded into micropores of the down feather, and the phase-change microcapsules can adjust the temperature of the down feather by absorbing / releasing heat.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of textiles, and in particular to down based on phase change heat storage and temperature regulation, a preparation method of the down, and the application of the down in the field of textiles. Background Art

[0002] Down is a mixture of "feather" and "down", and is an animal protein fiber. Down is the down cluster, which is the essence and value of down. Down cluster is a down core that radiates many down fibers and forms a three-dimensional cluster structure. Down fibers are composed of countless tiny hair scales. Each down fiber is densely covered with thousands of triangular tiny pores, which can shrink and expand with the temperature change, produce the function of warming and storing heat, absorb the flowing heat emitted by the human body, and isolate the invasion of cold air from the outside. The three-dimensional structure of down determines the comfort and fluffiness of down. There will be no problem of caking, and it will remain fluffy after long-term use. Down products are characterized by light weight, soft texture and good warmth retention.

[0003] Traditional down relies on heat reflection and heat insulation to achieve thermal insulation and comfort. The heat retention performance and temperature comfort after single heat storage cannot be adjusted in time. The existing processing procedures for down cannot give down the functionality of self-temperature regulation based on the characteristics of down fluff. Summary of the invention

[0004] In order to solve at least one of the above technical problems, a down that can adjust its temperature by itself is developed. The present application provides down based on phase change heat storage and temperature regulation, a preparation method of the down, and application of the down in the field of textiles.

[0005] On the one hand, the present application provides a down based on phase change heat storage and temperature regulation, wherein a phase change material is attached to the surface of the down and / or adsorbed in the pores; the phase change material is fully / partially embedded in the micropores of the down; the phase change material is made of the following components:

[0006] Phase change microcapsules 40-60wt%;

[0007] Attapulgite 35-45wt%;

[0008] Graphene oxide 5-15wt%.

[0009] By adopting the above technical solution, the phase change material composed of phase change microcapsules, attapulgite, and graphene oxide is fully / partially embedded in the micropores of the down, and the phase change microcapsules can adjust the temperature of the down by absorbing / releasing heat. Graphene oxide and phase change microcapsules are fully / partially embedded in the porous channels of attapulgite. In a dry environment, the combination of attapulgite and graphene can effectively reduce the generation of static electricity, and can make the phase change material difficult to separate from the down through the attraction of positive and negative charges. In a humid environment or during the washing process, the hygroscopic and expanding characteristics of attapulgite are used to fix the phase change material in the micropores of the down and make it difficult to fall off; and the expansion of attapulgite in the micropores or gaps of the down can reduce the reduction of the size of the micropores of the down, thereby ensuring the thermal insulation performance of the down.

[0010] Optionally, the wall material of the phase change microcapsule is silicon dioxide.

[0011] Optionally, the core material of the phase change microcapsule is paraffin.

[0012] Optionally, the particle size of the attapulgite is 0.2 to 1 μm.

[0013] Optionally, the parameters of the graphene oxide are: diameter 0.01 μm to 15 μm, thickness 0.55 nm to 3.85 nm, number of layers <10, purity >99% wt.

[0014] In a second aspect, the present application provides a method for preparing the above-mentioned down, comprising the following steps:

[0015] S1, mixing attapulgite and graphene oxide to obtain a mixture;

[0016] S2, mixing the mixture with phase change microcapsules to obtain a phase change material;

[0017] S3. Mixing the phase change material with the down, so that the phase change material is fully / partially embedded in the micropores of the down.

[0018] Optionally, in S1, the mixing conditions of attapulgite and graphene oxide are: temperature ≥ 100°C, air humidity ≥ 100%, and pressure greater than 0.1 MPa.

[0019] Optionally, in S2, the mixing conditions of the compound and the phase change microcapsules are: room temperature, air humidity ≥ 100%, and pressure greater than 0.1 MPa.

[0020] Optionally, in S3, the down is charged with a positive charge by friction and then mixed with a phase change material.

[0021] In a third aspect, the present application provides the application of the above-mentioned down in the field of textiles.

[0022] In summary, the phase change material composed of phase change microcapsules, attapulgite, and graphene oxide is fully / partially embedded in the micropores of down, and the phase change microcapsules can adjust the temperature of the down by absorbing / releasing heat. Graphene oxide and phase change microcapsules are fully / partially embedded in the porous channels of attapulgite. In a dry environment, the combination of attapulgite and graphene can effectively reduce the generation of static electricity, and can make the phase change material difficult to separate from the down through the attraction of positive and negative charges. In a humid environment or during the washing process, the hygroscopic and expanding properties of attapulgite are utilized to fix the phase change material in the micropores of the down and make it difficult to fall off; and the expansion of attapulgite in the micropores or gaps of the down can reduce the reduction of the size of the micropores of the down, thereby ensuring the thermal insulation performance of the down. DETAILED DESCRIPTION

[0023] The present application provides a down feather with temperature regulation based on phase change heat storage, wherein a phase change material is attached to the surface of the down feather and / or adsorbed in the pores; the phase change material is fully / partially embedded in the micropores of the down feather;

[0024] The phase change material is made from the following components:

[0025] Phase change microcapsules 40-60wt%;

[0026] Attapulgite 35-45wt%;

[0027] Graphene oxide 5-15wt%.

[0028] The present application also provides a method for preparing the above-mentioned down, comprising the following steps:

[0029] S1, mixing attapulgite and graphene oxide to obtain a mixture;

[0030] S2, mixing the mixture with phase change microcapsules to obtain a phase change material;

[0031] S3. Mixing the phase change material with the down, so that the phase change material is fully / partially embedded in the micropores of the down.

[0032] The present application also provides applications of the down in the field of textiles, such as down jackets, down quilts, etc.

[0033] In order to achieve the function of self-temperature regulation of down, the applicant adsorbed phase change microcapsules on the surface of down, which can achieve the function of self-temperature regulation and change the temperature regulation range according to the selection of phase change microcapsules. However, during the continuous vibration and washing process, the phase change microcapsules continuously fall off from the surface of the down, thus losing the self-temperature regulation function. Therefore, the applicant considered reducing the size of the phase change microcapsules and adsorbing them in the micropores on the surface of the down, thereby reducing the proportion of them falling off from the surface of the down; but the effect is not very obvious.

[0034] Therefore, after continuous attempts, the applicant discovered that the use of nano-scale attapulgite can utilize its unique and abundant channels to fix the phase change microcapsules, and the rough surface of the attapulgite itself can be better fixed in the micropores on the surface of the down, and the attapulgite has hygroscopicity and swelling properties. The hygroscopicity can reduce the generation of static electricity, and the swelling property makes the attapulgite larger in size after absorbing moisture, and better fixed in the micropores on the surface of the down.

[0035] In order to further fix the phase change material, the applicant added a small amount of graphene oxide, which was fully / partially embedded in the channels of the attapulgite, thereby enhancing the flow of electrons between the down and the phase change material and reducing the micropores on the surface of the down that cause the phase change material to detach from the down due to charge repulsion. The addition of graphene oxide can further reduce the generation of static electricity.

[0036] The present application is further described in detail below with reference to the embodiments.

[0037] In the following examples of the present application, the main components involved, unless otherwise specified, were purchased from commercially available products.

[0038] Phase change microcapsules: purchased from Hefei Ruixue New Material Technology Co., Ltd., the wall material is made of silicon dioxide, the core material is paraffin, and the melting point is 28°C; the phase change microcapsules here are not the only choice. The applicant chose it after considering the difficulty, cost and effect of making it in a size of 0.5-10μm. The use of silicon dioxide as the wall material can make the heat conduction faster; the melting point of 28°C is based on the consideration that when down jackets and down quilts are used by normal people, this temperature will be more comfortable. If it is used as a textile for other purposes or as an application in special scenarios, other melting points can be selected, such as 37°C. Specific embodiments

[0040] Example 1

[0041] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0042] The phase change material used in this embodiment includes: 40wt% of phase change microcapsules; 45wt% of attapulgite; and 15wt% of graphene oxide.

[0043] Mixing attapulgite and graphene oxide at room temperature and pressure with an air humidity of 50% to obtain a mixture;

[0044] The mixture is mixed with phase change microcapsules at room temperature and pressure and with an air humidity of 50% to obtain a phase change material;

[0045] Excess phase change material is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0046] Example 2

[0047] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0048] The phase change material used in this embodiment includes: 45 wt % of phase change microcapsules; 42 wt % of attapulgite; and 13 wt % of graphene oxide.

[0049] Mixing attapulgite and graphene oxide at room temperature and pressure with an air humidity of 50% to obtain a mixture;

[0050] The mixture is mixed with phase change microcapsules at room temperature and pressure and with an air humidity of 50% to obtain a phase change material;

[0051] Excess phase change material is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0052] Example 3

[0053] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0054] The phase change material used in this embodiment includes: 50wt% of phase change microcapsules; 40wt% of attapulgite; and 10wt% of graphene oxide.

[0055] Mixing attapulgite and graphene oxide at room temperature and pressure with an air humidity of 50% to obtain a mixture;

[0056] The mixture is mixed with phase change microcapsules at room temperature and pressure and with an air humidity of 50% to obtain a phase change material;

[0057] Excess phase change material is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0058] Example 4

[0059] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0060] The phase change material used in this embodiment includes: 55 wt % of phase change microcapsules; 38 wt % of attapulgite; and 7 wt % of graphene oxide.

[0061] Mixing attapulgite and graphene oxide at room temperature and pressure with an air humidity of 50% to obtain a mixture;

[0062] The mixture is mixed with phase change microcapsules at room temperature and pressure and with an air humidity of 50% to obtain a phase change material;

[0063] Excess phase change material is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0064] Example 5

[0065] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0066] The phase change material used in this embodiment includes: 60wt% of phase change microcapsules; 35wt% of attapulgite; and 5wt% of graphene oxide.

[0067] Mixing attapulgite and graphene oxide at room temperature and pressure with an air humidity of 50% to obtain a mixture;

[0068] The mixture is mixed with phase change microcapsules at room temperature and pressure and with an air humidity of 50% to obtain a phase change material;

[0069] Excess phase change material is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0070] Example 6

[0071] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0072] The phase change material used in this embodiment includes: 40wt% of phase change microcapsules; 45wt% of attapulgite; and 15wt% of graphene oxide.

[0073] Mixing attapulgite and graphene oxide under an environment where the temperature is ≥100° C., the air humidity is ≥100%, and the pressure is greater than 0.1 MPa to obtain a mixture;

[0074] The mixture is mixed with phase change microcapsules at room temperature and pressure and with an air humidity of 50% to obtain a phase change material;

[0075] Excess phase change material is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0076] Example 7

[0077] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0078] The phase change material used in this embodiment includes: 45 wt % of phase change microcapsules; 42 wt % of attapulgite; and 13 wt % of graphene oxide.

[0079] Mixing attapulgite and graphene oxide at room temperature and pressure with an air humidity of 50% to obtain a mixture;

[0080] The mixture is mixed with phase change microcapsules at room temperature, air humidity ≥ 100%, and pressure greater than 0.1 MPa to obtain a phase change material;

[0081] Excess phase change material is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0082] Example 8

[0083] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0084] The phase change material used in this embodiment includes: 50wt% of phase change microcapsules; 40wt% of attapulgite; and 10wt% of graphene oxide.

[0085] Mixing attapulgite and graphene oxide at room temperature and pressure with an air humidity of 50% to obtain a mixture;

[0086] The mixture is mixed with phase change microcapsules at room temperature and pressure and with an air humidity of 50% to obtain a phase change material;

[0087] The down is stirred and rubbed with the material that comes after wool in the friction sequence (metal>synthetic fiber>cotton>wood>wool>rabbit hair>silk>paper>glass>crystal>human body) to make the down positively charged; attapulgite is positively charged under normal conditions, and excess phase change material is mixed with the down to further increase the amount of phase change material fully / partially embedded in the micropores of the down through the effect of charge attraction; thereby obtaining down based on phase change heat storage and temperature regulation.

[0088] Example 9

[0089] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0090] The phase change material used in this embodiment includes: 55 wt % of phase change microcapsules; 38 wt % of attapulgite; and 7 wt % of graphene oxide.

[0091] Mixing attapulgite and graphene oxide under an environment where the temperature is ≥100° C., the air humidity is ≥100%, and the pressure is greater than 0.1 MPa to obtain a mixture;

[0092] The mixture is mixed with phase change microcapsules at room temperature, air humidity ≥ 100%, and pressure greater than 0.1 MPa to obtain a phase change material;

[0093] Excess phase change material is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0094] Example 10

[0095] This embodiment provides a method for preparing down based on phase change heat storage and temperature regulation.

[0096] The phase change material used in this embodiment includes: 60wt% of phase change microcapsules; 35wt% of attapulgite; and 5wt% of graphene oxide.

[0097] Mixing attapulgite and graphene oxide under an environment where the temperature is ≥100° C., the air humidity is ≥100%, and the pressure is greater than 0.1 MPa to obtain a mixture;

[0098] The mixture is mixed with phase change microcapsules at room temperature, air humidity ≥ 100%, and pressure greater than 0.1 MPa to obtain a phase change material;

[0099] The down is stirred and rubbed with the material that comes after wool in the friction sequence (metal>synthetic fiber>cotton>wood>wool>rabbit hair>silk>paper>glass>crystal>human body) to make the down positively charged; attapulgite is positively charged under normal conditions, and excess phase change material is mixed with the down to further increase the amount of phase change material fully / partially embedded in the micropores of the down through the effect of charge attraction; thereby obtaining down based on phase change heat storage and temperature regulation.

[0100] Comparative Example 1

[0101] Excessive phase change material (phase change microcapsules) is mixed with down at normal temperature and pressure with an air humidity of 50% to obtain down with temperature regulation based on phase change heat storage.

[0102] According to GB / T 10288-2016, the fluffiness and weight of the down were tested before and after treatment. Before the weight of the treated down was tested, the down was soaked in water and rotated at a speed of 20 r / s for 1 min. After being taken out, it was blown at a wind speed of 4 to 5 m / s for 60 s (dried) at normal temperature and pressure and an air humidity of 50%. The results are shown in Table 1.

[0103] Table 1

[0104]

[0105] It can be seen from Examples 1 to 5, Comparative Example 1 and Table 1 that the technical solution of the present application can greatly increase the adhesion rate of the phase change material on the down, so that the preparation method of the present application can produce down that can store heat and regulate temperature by itself.

[0106] And it can be seen from Example 1, Example 6 and Table 1 that changing the mixing conditions of attapulgite and graphene oxide to: temperature ≥ 100°C, air humidity ≥ 100%, and pressure greater than 0.1 MPa can improve the effect on the fluffiness of down after treatment and further improve the adhesion rate of the phase change material.

[0107] It can be seen from Example 2, Example 7 and Table 1 that changing the mixing conditions of the mixture (attapulgite and graphene oxide) and the phase change microcapsules to: normal temperature, air humidity ≥ 100%, and pressure greater than 0.1 MPa can improve the effect on the fluffiness of down after treatment and further improve the adhesion rate of the phase change material.

[0108] It can be seen from Example 3, Example 8 and Table 1 that making the down have a positive charge and then mixing it with the phase change material can significantly improve the effect on the fluffiness of the down after treatment and increase the adhesion rate of the phase change material compared to Example 6 / 7.

[0109] It can be seen from Examples 6 to 10 and Table 1 that by simultaneously changing the mixing conditions of attapulgite and graphene oxide, the mixing conditions of the mixture and phase change microcapsules, and making the down positively charged and then mixing it with the phase change material, the effect on the fluffiness of the down after treatment can be improved in one step, thereby increasing the adhesion rate of the phase change material.

[0110] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A down feather based on phase change heat storage and temperature regulation, characterized in that: Phase change material is attached to the surface of the down and / or adsorbed in the pores; the phase change material is fully / partially embedded in the micropores of the down; The phase change material is made from the following components: Phase change microcapsules 40-60wt%; Attapulgite 35-45wt%; Graphene oxide 5-15wt%.

2. The down according to claim 1, characterized in that: The wall material of the phase change microcapsule is silicon dioxide.

3. The down according to claim 1, characterized in that: The core material of the phase-change microcapsule is paraffin.

4. The down according to claim 1, characterized in that: The particle size of the attapulgite is 0.2-1 μm.

5. The down according to claim 1, characterized in that: The parameters of the graphene oxide are: diameter 0.01 μm to 15 μm, thickness 0.55 nm to 3.85 nm, number of layers <10, purity >99% wt.

6. A method for preparing down according to claim 1, characterized in that: The following steps are involved: S1, mixing attapulgite and graphene oxide to obtain a mixture; S2, mixing the mixture with phase change microcapsules to obtain a phase change material; S3. Mixing the phase change material with the down, so that the phase change material is fully / partially embedded in the micropores of the down.

7. The preparation method according to claim 6, characterized in that: In S1, the mixing conditions of attapulgite and graphene oxide are: temperature ≥ 100°C, air humidity ≥ 100%, and pressure greater than 0.1 MPa.

8. The preparation method according to claim 6, characterized in that: In S2, the mixing conditions of the mixture and the phase change microcapsules are: room temperature, air humidity ≥ 100%, and pressure greater than 0.1 MPa.

9. The preparation method according to claim 6, characterized in that: In S3, the down is charged with positive charges by friction and then mixed with the phase change material.

10. Use of the down according to claim 1 in the field of textiles.