Large-tow carbon fiber multifilament tensile test sample and preparation method thereof

By applying tension to large tow carbon fibers and phased heating and curing methods, combined with the use of epoxy adhesives, the discretency and defect problems of the tensile test of large tow carbon fibers are solved, and the accuracy and stability of the test are improved.

CN118937043APending Publication Date: 2024-11-12BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411066588.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art lacks tensile performance testing standards for large tow carbon fibers, resulting in large discreteness and sample defects in the test results.

Method used

The large tow carbon fiber is wound on the wire winding rack to apply tension, and then soaked in the epoxy resin solution to perform heating and curing in stages. Combined with the reinforcement sheet of epoxy adhesive and pressurized curing, a large tow carbon fiber composite is prepared. Wire tensile test specimens.

Benefits of technology

It effectively avoids the torsion and uneven force of the fiber bundle, reduces the occurrence of internal cavity, improves the accuracy and stability of tensile tests, and reduces sample defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937043A_ABST
    Figure CN118937043A_ABST
Patent Text Reader

Abstract

The invention discloses a large-tow carbon fiber multifilament tensile test sample and a preparation method thereof, and the method comprises the following steps: (1) winding large-tow carbon fibers on a rectangular filament winding frame, and applying 60N-80N tension to the large-tow fibers; (2) immersing the filament winding frame wound with the carbon fiber filament bundle obtained in the step (1) into a glue box filled with an epoxy resin solution; (3) the multifilament soaked with the glue solution obtained in the step (2) is subjected to heating curing in an air dry oven, heating curing comprises a first stage and a second stage, the temperature of the first stage is 30-50 DEG C, and the constant temperature time is 0.5-1 h; the temperature of the second stage is 100-130 DEG C, and the constant temperature time is 3-4 hours; and (4) cutting the cured large-tow carbon fiber multifilament sample strip obtained in the step (3), coating a reinforcing sheet with an epoxy adhesive, adhering the epoxy adhesive to two ends of the large-tow carbon fiber multifilament sample strip along the length direction of the cured large-tow carbon fiber multifilament sample strip, heating and curing under a pressurizing condition, and cooling to obtain the large-tow carbon fiber multifilament tensile test sample.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material performance testing, and in particular relates to a large-tow carbon fiber multifilament tensile test specimen and a preparation method thereof. Background Art

[0002] Carbon fiber has excellent mechanical properties such as light weight and high strength, as well as functional properties such as electrical conductivity, thermal conductivity, and corrosion resistance. Therefore, advanced composite materials using it as reinforcement are widely used in aerospace, clean energy, transportation, industrial construction, sports and leisure, etc. As a load-bearing material in the structure, the tensile properties of carbon fiber are usually the focus of research. Therefore, it is particularly important to evaluate the tensile strength of carbon fiber multifilaments through tensile testing.

[0003] At present, the tensile performance test methods of small-tow carbon fibers (1k, 6k, 12, 24k) are all carried out in accordance with the national standard GB / T 3362-2017. There is a lack of relevant test standards for large-tow carbon fibers (48k and above). The tensile performance test of large-tow carbon fibers based on GB / T 3362-2017 has considerable discreteness.

[0004] Therefore, the existing large-tow carbon fiber tensile test needs to be improved. Summary of the invention

[0005] The invention provides a large-tow carbon fiber multifilament tensile test specimen and a preparation method thereof. The method can solve the current problems of large-tow carbon fiber multifilament having many defects and large dispersion of tensile test performance.

[0006] The present invention provides a method for preparing a large-tow carbon fiber multifilament tensile test specimen, comprising:

[0007] (1) Winding a large tow carbon fiber on a rectangular winding frame, and applying a tension of 60N-80N to the large tow fiber;

[0008] (2) immersing the winding frame for winding the carbon fiber tow obtained in step (1) in a plastic box containing an epoxy resin solution;

[0009] (3) placing the multifilaments soaked in the glue obtained in step (2) in a blast drying oven for heating and curing, wherein the heating and curing comprises a first stage and a second stage: the temperature of the first stage is 30 to 50° C. and the time is 0.5 to 1 hour; the temperature of the second stage is 100 to 130° C. and the time is 3 to 4 hours;

[0010] (4) Cut the solidified large-tow carbon fiber multifilament strip obtained in step (3), apply epoxy adhesive on the reinforcing sheet and stick it on both ends along the length direction of the solidified large-tow carbon fiber multifilament strip, place it in an oven under pressure to heat and solidify, and obtain a large-tow carbon fiber multifilament tensile test specimen after cooling.

[0011] Furthermore, in step (1), the tow of the large-tow carbon fiber is not less than 48K.

[0012] Furthermore, in step (2), the epoxy resin solution comprises epoxy resin, curing agent, accelerator and solvent, and the mass ratio of the epoxy resin, curing agent, accelerator and solvent is 100:75-90:1-3:(100-130).

[0013] Further, the epoxy resin includes at least one of E51, E44, AG-80 and TDE85.

[0014] Furthermore, the curing agent includes at least one of methyl tetracyanophthalic anhydride, methyl hexacyanophthalic anhydride and methyl nadic anhydride.

[0015] Furthermore, the accelerator includes at least one of 2,4,6-tris(dimethylaminomethyl)phenol, dimethylbenzylamine, and imidazole.

[0016] Furthermore, in step (4), the epoxy adhesive includes J-22 adhesive.

[0017] Furthermore, in step (4), the pressurized pressure is 1600Pa-2000Pa.

[0018] Furthermore, in step (4), the curing temperature is 120-140°C.

[0019] The second aspect of the present invention discloses a large-tow carbon fiber multifilament tensile test specimen obtained by the above method.

[0020] Compared with the prior art: the preparation method proposed in the present invention can avoid the torsion of the fiber bundle and the uneven force in the bundle by applying a tension of 60N-80N to the large-tow carbon fiber wound on the winding frame, thereby reducing the situation where the fibers in the sample cannot bear the force at the same time due to bending; then the multifilaments immersed in the glue solution are heated in the first stage and the second stage in sequence. A lower temperature is used in the first stage, which can guide the volatilization of the solvent in the fiber bundle soaked in the epoxy resin solution to avoid the resin solidifying too quickly during the second stage of curing and heating, resulting in the difficulty of the solvent to volatilize and produce internal voids in the multifilament spline, thereby solving the current problems of many defects in large-tow carbon fiber multifilaments and large dispersion of tensile test performance, and improving the accuracy and stability of tensile performance testing of large-tow carbon fiber multifilaments. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of a large-tow carbon fiber multifilament tensile test specimen of the present invention. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below in conjunction with examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0023] In one aspect of the present invention, the present invention provides a method for preparing a large-tow carbon fiber multifilament tensile test specimen, comprising the following steps:

[0024] S1: Winding large tow carbon fiber on a rectangular winding frame

[0025] In this step, a large tow carbon fiber of not less than 48k is wound on a rectangular winding frame, and the bundle width of the large tow carbon fiber is adjusted to avoid twisting of the fiber bundle, and a tension of 60N-80N is applied to the large tow fiber to ensure that the fiber bundle does not sag due to gravity after dipping, and to ensure that the fiber is straight. The inventor found that by applying a tension of 60N-80N to the large tow carbon fiber wound on the winding frame, the twisting of the fiber bundle and the uneven force in the bundle can be avoided, thereby reducing the situation where the fiber bending in the sample cannot bear the force at the same time, thereby improving the accuracy and stability of the tensile performance test of the large tow carbon fiber multifilament.

[0026] S2: Immerse the winding frame of the carbon fiber tow obtained in step S1 in a plastic box containing epoxy resin solution.

[0027] Specifically, in the embodiment of the present invention, the plastic box containing the epoxy resin solution is first stirred and heated (15-25°C, heated for 8-15 minutes) to ensure the uniformity and good fluidity of the epoxy resin solution, and then the winding frame for winding the carbon fiber bundle obtained in step S1 is immersed in the plastic box containing the epoxy resin solution, that is, the resin solution must immerse the entire winding frame to avoid insufficient infiltration of the fiber bundle and the resin due to insufficient resin solution.

[0028] Furthermore, the epoxy resin solution comprises epoxy resin, curing agent, accelerator and solvent, and the mass ratio of the epoxy resin, curing agent, accelerator and solvent is 100:75-90:1-3:(100-130).

[0029] Furthermore, the epoxy resin includes but is not limited to at least one of E51, E44, AG-80 and TDE85; the curing agent includes but is not limited to at least one of methyl tetracyanophthalic anhydride, methyl hexacyanophthalic anhydride and methyl nadic anhydride; the accelerator includes but is not limited to at least one of 2,4,6-tris(dimethylaminomethyl)phenol, dimethylbenzylamine and imidazole; the solvent includes but is not limited to acetone.

[0030] S3: placing the multifilaments soaked in the glue obtained in step S2 in a blast drying oven to heat and solidify

[0031] In an embodiment of the present invention, the multifilaments soaked in the glue obtained in step S2 are placed in a blast drying oven for heating and curing, and the heating and curing includes a first stage and a second stage: the temperature of the first stage is 30-50°C, and the constant temperature time is 0.5-1 hour; the temperature of the second stage is 100-130°C, and the constant temperature time is 3-4 hours. Specifically, a lower temperature is used in the first stage, so that the solvent such as acetone in the fiber bundle soaked in the epoxy resin solution can be volatilized and guided out, so as to avoid the resin solidifying too fast during the curing and heating process in the second stage, which makes it difficult for the solvent to volatilize and produce internal voids in the multifilament spline. The temperature of the second stage is 100-130°C, and the constant temperature time is 3-4 hours, so that the epoxy resin in the glue can be fully cured and avoid excessive aging.

[0032] S4: Cut the solidified large-tow carbon fiber multifilament spline obtained in step S3, apply epoxy adhesive on the reinforcing sheet and stick it on both ends along the length direction of the solidified large-tow carbon fiber multifilament spline, place it in an oven under pressure to heat and solidify, and obtain a large-tow carbon fiber multifilament tensile test specimen after cooling.

[0033] According to an embodiment of the present invention, the reinforcing sheets and the cured multifilaments are cut according to the dimensions required by GB / T 3362-2017. For example, the reinforcing sheets at both ends of the sample are 50 mm long and 20 mm wide. The test section of the sample is 150 mm. The reinforcing sheets are made of kraft paper with a thickness of 1 to 2 mm. The large-tow carbon fiber multifilament splines after cutting and curing are preferably flat, flat and straight. If the multifilament splines cut by the large-tow carbon fiber dipping and curing are round rods, most of the splines are found to have large cavities inside after being cut transversely, resulting in large defects in the large-tow carbon fiber multifilament test specimens. During the tensile loading process, they may be broken due to the clamping pressure, affecting the results of the tensile test performance.

[0034] Furthermore, the epoxy adhesive includes J-22 adhesive; and the pressurized pressure is 1600Pa-2000Pa; and the curing temperature is 120-140° C. Specifically, the two ends of the fiber multifilament sample are usually not flat surfaces, so applying the above pressure can make the epoxy adhesive fully contact with the fiber multifilament and the reinforcement sheet, thereby increasing the contact area, improving the bonding effect, and avoiding the reinforcing sheet from slipping during the test loading process.

[0035] Therefore, the method of the present invention can solve the current problems of large-tow carbon fiber multifilaments having many defects and large dispersion of tensile test performance.

[0036] The second aspect of the present invention discloses a large-tow carbon fiber multifilament tensile test specimen obtained by the above method.

[0037] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0038] Example 1

[0039] (1) The tensile properties of a domestically produced T700-grade 48k large-tow carbon fiber were tested. First, a 2-meter-long section of large-tow carbon fiber was taken from the wire roller, and the torsion of the fiber tow was adjusted to make it flat. The free end was fixed on the winding frame, and a certain tension force (applying a tension of 70N) was controlled to tension the carbon fiber tow on the winding frame. The standard was that the force on each part of the tow was uniform and there was no partial relaxation.

[0040] (2) epoxy resin E51, curing agent methyl hexacyanoanhydride and accelerator dimethylbenzylamine are uniformly dissolved in acetone in a mass ratio of 100:75:2 to obtain an epoxy resin solution, the obtained epoxy resin solution is poured into a glue box, the glue box containing the epoxy resin solution is stirred and heated (20° C., 10 minutes), and then the winding frame for winding carbon fiber tow obtained in step (1) is immersed in the glue box containing the epoxy resin solution for 3-5 minutes, and then the glue-soaked winding frame is taken out and the excess epoxy resin solution on the multifilament is sucked off with glue-absorbing paper to achieve a draining effect;

[0041] (3) placing the multifilaments soaked in the glue obtained in step (2) into a blast drying oven for a staged heating process, firstly setting the temperature at 40° C. for 30 min in the first stage to allow the acetone solvent to evaporate rapidly at a temperature below its boiling point without affecting the subsequent second stage resin curing, and then raising the temperature to 120° C. for 3 h in the second stage for resin curing;

[0042] (4) Cut the winding frame after curing in step (3) into carbon fiber multifilaments of about 250 mm in length, select carbon fiber multifilament splines that are flat, straight and free of hair on the surface, take an appropriate amount of J-22 resin binder (the mass ratio of A and B components is 1:1, provided by the Institute of Petroleum Chemistry of Heilongjiang Academy of Sciences) with a ratio of 1:1 and apply it on the surface of the wire. Figure 1 The reinforcing sheet (the reinforcing sheet is 50 mm long, 20 mm wide, the sample test section is 150 mm, the reinforcing sheet is made of kraft paper, and the thickness is 2 mm) is positioned, and pressure is applied to the reinforcing sheet in a direction perpendicular to the length of the carbon fiber (the pressure range is 1800 Pa), and placed in a blast drying oven at a constant temperature of 130°C for 2 hours for curing; after natural cooling, it is cut into the following Figure 1 The large-tow carbon fiber multifilament tensile test specimens shown, 8 groups of tensile property test results of this embodiment 1 are shown in Table 1.

[0043] Example 2

[0044] The tensile properties of the domestically produced T700-grade 48k large-tow carbon fiber in Example 1 were tested. The other steps were the same as in Example 1, except that in step (1), a section of about 5 m of the large-tow carbon fiber was first cut from the wire roller, the torsion of the fiber bundle was manually adjusted to make it flat, and the section of the carbon fiber bundle was wound on a new roller, and then the fiber bundle was framed. The results of the 8 groups of tensile properties tests in this example are shown in Table 1.

[0045] Example 3

[0046] The tensile properties of Formosa Plastics TC-35R brand 48k large tow carbon fiber were tested; the other steps were the same as in Example 1, and the results of the 8 groups of tensile properties tests in this example are shown in Table 1.

[0047] Example 4

[0048] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 2, and the results of the 8 groups of tensile properties tests in this example are shown in Table 1.

[0049] Example 5

[0050] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the temperature of the first stage of the heating and curing process in step (3) was 30°C, and the constant temperature time was 1 hour.

[0051] Example 6

[0052] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the temperature of the first stage of the heating and curing process in step (3) was 50°C, and the constant temperature time was 0.5 hours.

[0053] Example 7

[0054] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the temperature of the second stage of the temperature-raising curing process in step (3) was 100°C and the constant temperature time was 4 hours.

[0055] Example 8

[0056] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the temperature of the second stage of the heating and curing process in step (3) was 130°C, and the constant temperature time was 3 hours.

[0057] Comparative Example 1

[0058] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the first stage was eliminated in step (3), and the temperature was directly raised to 120°C and kept constant for 3 hours for resin curing. The results of the 8 groups of tensile properties tests of Comparative Example 1 are shown in Table 1.

[0059] Comparative Example 2

[0060] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 2, except that the first stage was eliminated in step (3), and the temperature was directly raised to 120°C and kept constant for 3 hours for resin curing. The results of the 8 groups of tensile properties tests in this example are shown in Table 1.

[0061] Comparative Example 3

[0062] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as those in Comparative Example 4, except that the first stage was eliminated in step (3), and the temperature was directly raised to 120°C and kept constant for 3 hours for resin curing. The results of the 8 groups of tensile properties tests in this Example are shown in Table 1.

[0063] Comparative Example 4

[0064] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested. The other steps were the same as in Example 1, except that the fiber was wound around the frame using a traditional method in step (1), i.e., the tension was controlled by pulling with fingers (the tension value was 20-30N). The results of the 8 groups of tensile properties tests in this example are shown in Table 1.

[0065] Comparative Example 5

[0066] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the temperature of the first stage of the heating and curing process in step (3) was 25°C, and the constant temperature time was 2 hours.

[0067] Comparative Example 6

[0068] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the temperature of the first stage of the heating and curing process in step (3) was 60°C, and the constant temperature time was 0.5 hours.

[0069] Comparative Example 7

[0070] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the temperature of the second stage of the heating and curing process in step (3) was 90°C and the constant temperature time was 5 hours.

[0071] Comparative Example 8

[0072] The tensile properties of the Formosa Plastics TC-35R brand 48k large-tow carbon fiber in Example 3 were tested; the other steps were the same as in Example 1, except that the temperature of the second stage of the heating and curing process in step (3) was 140°C, and the constant temperature time was 3 hours.

[0073] The tensile test specimens obtained in the above embodiments and comparative examples were tested using INSTRON-5966 equipment (the test scheme refers to GB / T 3362-2017). Eight groups of specimens were taken for each embodiment and comparative example. The average values ​​of the eight groups of specimens are shown in Table 1, and the dispersion (CV) of the test results of the comparative example specimens of each embodiment is shown in Table 1.

[0074] Table 1

[0075]

[0076]

[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a large-tow carbon fiber multifilament tensile test specimen, characterized in that: include: (1) Winding a large tow carbon fiber on a rectangular winding frame, and applying a tension of 60N-80N to the large tow fiber; (2) immersing the winding frame for winding the carbon fiber tow obtained in step (1) in a plastic box containing an epoxy resin solution; (3) placing the multifilaments soaked in the glue obtained in step (2) in a blast drying oven for heating and curing, wherein the heating and curing comprises a first stage and a second stage: the temperature of the first stage is 30 to 50° C., and the constant temperature time is 0.5 to 1 hour; the temperature of the second stage is 100 to 130° C., and the constant temperature time is 2 to 3 hours; (4) Cut the solidified large-tow carbon fiber multifilament strip obtained in step (3), apply epoxy adhesive on the reinforcing sheet and stick it on both ends along the length direction of the solidified large-tow carbon fiber multifilament strip, place it in an oven under pressure to heat and solidify, and obtain a large-tow carbon fiber multifilament tensile test specimen after cooling.

2. The method according to claim 1, characterized in that In step (1), the tow of the large-tow carbon fiber is not less than 48K.

3. The method according to claim 1 or 2, characterized in that: In step (2), the epoxy resin solution comprises epoxy resin, curing agent, accelerator and solvent, and the mass ratio of the epoxy resin, curing agent, accelerator and solvent is 100:75-90:1-3:(100-130).

4. The method according to claim 3, characterized in that The epoxy resin includes at least one of E51, E44, AG-80 and TDE85.

5. The method according to claim 3, characterized in that: The curing agent includes at least one of methyl tetracyanophthalic anhydride, methyl hexacyanophthalic anhydride and methyl nadic anhydride.

6. The method according to claim 3, characterized in that The accelerator includes at least one of 2,4,6-tris(dimethylaminomethyl)phenol, dimethylbenzylamine and imidazole.

7. The method according to claim 1, characterized in that In step (4), the epoxy adhesive includes J-22 adhesive.

8. The method according to claim 1 or 7, characterized in that: In step (4), the pressurized pressure is 1600Pa-2000Pa.

9. The method according to claim 1 or 7, characterized in that: In step (4), the curing temperature is 120°C-140°C.

10. A large-tow carbon fiber multifilament tensile test specimen prepared by the method according to any one of claims 1 to 9.