Sea urchin-shaped Au-coated Pd nano material, hydrogen sensor and preparation method of hydrogen sensor

By preparing sea urchin-shaped Au@Pd nanomaterials, the problem of large volume and low sensitivity of hydrogen sensors is solved, and a small volume and high sensitivity of hydrogen detection is achieved to meet the detection needs of narrow spaces.

CN118937260APending Publication Date: 2024-11-12CHENGDU SCI & TECH DEV CENT CHINA ACAD OF ENG PHYSICS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411015115.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing hydrogen sensors are large in size and have low sensitivity, which cannot meet the requirements for hydrogen detection in a narrow space.

Method used

Using sea urchin-shaped Au@Pd nanomaterials, control the ratio and reaction temperature of Au nanoparticles, palladium chloric acid and cetyl trimethylammonium chloride, nanomaterials with a larger specific surface area are prepared for hydrogen sensors. , realize small-volume and high-sensitivity hydrogen detection.

Benefits of technology

It achieves fast response less than 2 seconds and a low detection limit of 0.1%, meeting the hydrogen detection needs in a narrow space, and solving the problems of large size and low sensitivity of traditional sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937260A_ABST
    Figure CN118937260A_ABST
Patent Text Reader

Abstract

The invention provides a sea urchin-shaped Au-coated Pd nano material, a hydrogen sensor and a preparation method of the sea urchin-shaped Au-coated Pd nano material, Au nano particles and palladium chlorate are used as main reaction raw materials, L-ascorbic acid is used as a reducing agent, hexadecyl trimethyl ammonium chloride is used as an additive, and by controlling the adding proportion and the reaction temperature of the raw materials, the prepared Au-coated Pd nano material is in a sea urchin shape; compared with Pd layers in other shapes, the Pd layer has a larger specific surface area, namely more reaction active sites, is used in a hydrogen sensor, can control the smaller volume of the sensor, realizes hydrogen detection with quick response and low detection limit, and meets the hydrogen detection requirement in a narrow space range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sensors, and in particular to a sea urchin-shaped Au@Pd nanomaterial, a hydrogen sensor and a preparation method thereof. Background Art

[0002] Hydrogen is an efficient, renewable, pollution-free secondary clean energy carrier with a wide range of sources. With the vigorous development of hydrogen production technology, hydrogen storage technology and hydrogen fuel cells, the large-scale use of hydrogen energy has become an urgent goal pursued by the world. In terms of renewable energy and clean energy, hydrogen (H2) has the greatest potential for utilization and can prevent harmful air pollution problems associated with traditional fuel sources. However, H2 is a colorless, odorless, flammable and explosive gas that cannot be detected by the human eye and nose even in high concentrations. More importantly, H2 has low ignition energy, high diffusion coefficient and wide explosion limit, which may lead to catastrophic consequences in the event of an accidental leak.

[0003] At present, hydrogen sensors on the market are classified into MEMS semiconductor type, MEMS catalytic type and electrochemical type based on the sensing principle. Unfortunately, MEMS semiconductor type and MEMS catalytic type hydrogen sensors cannot be exposed to silicone rubber systems and places where volatile silicon compounds exist. The main reason is that volatile silicon compound vapor will be produced in the above systems and places. The silicon compound vapor will condense a thin film on the surface of the hydrogen sensor, causing physical barriers, making it impossible to identify hydrogen-philic molecules, resulting in the inability of hydrogen sensing to accurately reflect the hydrogen concentration in the measured place. Electrochemical hydrogen sensors are relatively large in size, with a height of more than 1 cm and a diameter of about 2 cm. Such a large volume cannot be designed and integrated in a small space such as a foam pad.

[0004] Therefore, it is of great significance to develop a hydrogen sensor with small size, high sensitivity and wide detection range for hydrogen detection in a narrow space. Summary of the invention

[0005] The purpose of the present invention is to provide a sea urchin-shaped Au@Pd nanomaterial, a hydrogen sensor and a preparation method thereof, in view of the problem that the existing hydrogen sensor has a large volume, low sensitivity, and a narrow detection range, and cannot meet the requirements of hydrogen detection in a narrow space. Au nanoparticles and palladium chloride are used as the main reaction raw materials, L-ascorbic acid is used as a reducing agent, and hexadecyltrimethylammonium chloride is used as an additive. By controlling the addition ratio of the raw materials and the reaction temperature, the prepared Au@Pd nanomaterial is in the shape of a sea urchin. Compared with other shapes of Pd layers, the material has a larger specific surface area, that is, more reactive sites. When used in a hydrogen sensor, the volume of the sensor can be controlled to be smaller, and ultra-sensitive (less than 2s) and low detection limit (0.1%) hydrogen detection can be achieved, which meets the requirements of hydrogen detection in a narrow space and achieves unexpected results.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a sea urchin-shaped Au@Pd nanomaterial comprises the following steps:

[0008] Step 1, adding Au nanoparticles, palladium chloride (H2PdCl4), and L-ascorbic acid into a hexadecyltrimethylammonium chloride (CTAC) aqueous solution and mixing well;

[0009] Step 2, controlling the temperature of the mixture obtained in step 1 to 34-38° C., and performing a heat-retention reaction to obtain a sea urchin-shaped Au@Pd nanomaterial;

[0010] The molar amount of hexadecyltrimethylammonium chloride added is 3.5×10 of the molar amount of Au nanoparticles added. 3 times or more;

[0011] The molar ratio of Au nanoparticles to palladium chloride is 1:1.6-8.

[0012] The invention provides a method for preparing a sea urchin-shaped Au@Pd nanomaterial. Au nanoparticles and palladium chloride are used as main reaction raw materials, L-ascorbic acid is used as a reducing agent, and hexadecyltrimethylammonium chloride is used as an additive. By controlling the addition ratio of the raw materials and the reaction temperature, the prepared Au@Pd nanomaterial is in the shape of a sea urchin. Compared with Pd layers of other shapes, the material has a larger specific surface area, that is, more reactive sites. The material is used in a hydrogen sensor, can control the volume of the sensor to be smaller, realizes ultra-sensitive (less than 2s) and low detection limit (0.1%) hydrogen detection, meets the hydrogen detection requirements in a narrow space, and achieves unexpected effects.

[0013] Furthermore, the molar ratio of Au nanoparticles to hexadecyltrimethylammonium chloride is 1:3.5×10 3 ~4.5×10 3In the preparation of Au@Pd nanomaterials, the present invention specifically adds hexadecyltrimethylammonium chloride. The addition of CTAC can adjust the affinity of the surface of the nanoparticles, so that the microscopic surface of the Au@Pd nanomaterial appears thorny. It is used in the preparation of hydrogen sensors and shows good effects. Preferably, the molar ratio of Au nanoparticles to hexadecyltrimethylammonium chloride is 1:4.0×10 3 ~4.5×10 3 .

[0014] Furthermore, the molar ratio of palladium chloride and L-ascorbic acid added is 2 to 3:1.

[0015] Furthermore, the molar ratio of Au nanoparticles to palladium chloroacid is 1:2-8. The addition ratio of palladium chloroacid is related to the thickness of the Pd layer formed in the sea urchin-shaped Au@Pd nanomaterial. Pd layers of different thicknesses will make the sensor have different sensitivities to hydrogen and different recognizabilities. The thicker the Pd layer, the greater the decrease in the absorbance of the sensor. This is because the more the dielectric constant of the environment around the Au nucleus changes, the more obvious the change in the Au plasma resonance peak, and the higher its recognizability. However, the Pd layer will also cause the response time to increase. This is because the diffusion of hydrogen requires a certain amount of time. A Pd layer that is too long will increase the response time. It is particularly important to note that a Pd layer that is too thin will provide too few active reaction sites, which will result in a long response time and unclear changes in the Au plasma resonance peak. Preferably, the molar ratio of Au nanoparticles to palladium chloroacid is 1:3-6.

[0016] Furthermore, before step 1, the Au nanoparticles are centrifugally washed using a hexadecyltrimethylammonium chloride aqueous solution to avoid the presence of impurities in the preparation process of the Au@Pd nanomaterial, which may affect the product performance.

[0017] Furthermore, Au nanoparticles are prepared by the following method:

[0018] S1, mixing chloroauric acid (HAuCl4), cetyltrimethylammonium bromide (CTAB), and sodium borohydride (NaBH4) and letting it stand to obtain an Au seed solution;

[0019] S2. Add the Au seed solution prepared in step S1 to an aqueous solution containing CTAB, chloroauric acid, and L-ascorbic acid (L-AA), shake and allow to react, and centrifuge to remove the supernatant to obtain Au nanoparticles.

[0020] Furthermore, in S1, the molar ratio of chloroauric acid, hexadecyltrimethylammonium bromide and sodium borohydride is 1:20-25:2-2.5.

[0021] Furthermore, in S2, the molar ratio of Au atoms, CTAB, chloroauric acid, L-ascorbic acid, and water in the Au seed solution is 1-3:2×10 5 ~2.5×10 5 :2.5×10 3 ~3.5×10 3 :1×10 4 ~2×10 4 :1.

[0022] Furthermore, in S1, the standing time is 1 to 3 hours.

[0023] Furthermore, in S2, the static reaction time is more than 12 hours, preferably, in S2, the static reaction time is 12 to 18 hours.

[0024] Furthermore, in step 2, the temperature of the mixed material obtained in step 1 is controlled at 35-36° C. Studies have found that the reaction temperature in the preparation of Au@Pd nanomaterials is a key factor affecting the performance of the material. If the reaction temperature is too low or too high, the growth state of the nanoparticles may be poor and the performance of the nanomaterial may be significantly reduced.

[0025] Furthermore, in step 2, the insulation reaction time is 12 to 16 hours.

[0026] Another object of the present invention is to provide a sea urchin-shaped Au@Pd nanomaterial prepared by the above preparation method.

[0027] A sea urchin-shaped Au@Pd nanomaterial prepared by the method for preparing the sea urchin-shaped Au@Pd nanomaterial.

[0028] Another object of the present invention is to provide a hydrogen sensor comprising the sea urchin-shaped Au@Pd nanomaterial.

[0029] A hydrogen sensor is prepared by using the sea urchin-shaped Au@Pd nanomaterial.

[0030] A method for preparing a hydrogen sensor comprises the following steps:

[0031] A1. Add the above-mentioned sea urchin-shaped Au@Pd nanomaterial into a perfluorodecanethiol solution, mix, and let stand; wherein the perfluorodecanethiol solution uses a mixture of ethanol and n-hexane as a solvent;

[0032] A2. After the n-hexane evaporates, Au@Pd nanoparticles are loaded onto the substrate using a glass slide to obtain a hydrogen sensor.

[0033] The present invention provides a method for preparing a hydrogen sensor, wherein sea urchin-shaped Au@Pd nanoparticles are self-liquid-loaded in a perfluorodecanethiol solution containing ethanol and n-hexane as solvents, and a uniform nanoparticle film is formed on a glass slide / PET / optical fiber substrate by an immersion and pulling method, thereby obtaining a sea urchin-shaped Au@Pd nanoarray hydrogen sensor. The plasma resonance peak of Au in the sensor containing perfluorodecanethiol will not change after hydrogen reaction, and the absorbance at a certain wavelength is less affected when it is selected as a response, and the detection accuracy is higher.

[0034] Furthermore, before step A1, the urchin-shaped Au@Pd nanomaterial is centrifugally washed, dispersed in water, and then the washed material is added to a perfluorodecanethiol solution for mixing and allowed to stand. On the one hand, dispersion in water can reduce the content of CTAC to a certain extent, which can improve the effect of self-assembly; on the other hand, the presence of surface active agents such as CTAC will hinder the contact between hydrogen and Pd to a certain extent.

[0035] Furthermore, in A2, the perfluorodecanethiol solution uses a mixture of ethanol and n-hexane as solvent, wherein the volume ratio of ethanol to n-hexane is 1:1.5 to 2.5.

[0036] Furthermore, in A2, the concentration of the perfluorodecanethiol solution is 8 to 12 mM, and the volume ratio of the nanoparticles to the perfluorodecanethiol solution is 1:1.5 to 2.5. mM represents millimole per liter concentration.

[0037] Furthermore, in A3, the substrate is a glass slide, PET or optical fiber.

[0038] Furthermore, it also includes A4, after loading Au@Pd nanoparticles onto a thin substrate, spin coating polymethyl methacrylate (PMMA) using a spin coater, and drying to obtain a hydrogen sensor.

[0039] The present application provides a hydrogen sensor that forms a PMMA polymer layer of a certain thickness by spin coating, thereby achieving selective detection of hydrogen by the sensor and solving the problem of poor repeatability of the hydrogen sensor formed by self-assembly of nanoparticles.

[0040] Preferably, in A4, the rotation speed of the spin coater is 5000-6000 r / min, and the spin coating time is 25-40 s.

[0041] Preferably, in A4, the mass concentration of polymethyl methacrylate is 3% to 5%.

[0042] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0043] 1. The present invention provides a method for preparing a sea urchin-shaped Au@Pd nanomaterial, which uses Au nanoparticles and palladium chloride as main reaction raw materials, L-ascorbic acid as a reducing agent, and hexadecyltrimethylammonium chloride as an additive. By controlling the addition ratio of the raw materials and the reaction temperature, the prepared Au@Pd nanomaterial is in the shape of a sea urchin. Compared with Pd layers of other shapes, the material has a larger specific surface area, i.e., more reactive sites. When used in a hydrogen sensor, the sensor can be controlled to have a smaller volume, and hydrogen detection with a fast response (less than 2s) and a low detection limit (0.1%) can be achieved, thereby meeting the requirements for hydrogen detection in a narrow space and achieving unexpected results.

[0044] 2. The present invention provides a method for preparing a hydrogen sensor, wherein sea urchin-shaped Au@Pd nanoparticles are self-assembled in a perfluorodecanethiol solution containing ethanol and n-hexane as solvents, and a uniform nanoparticle film is formed on a glass slide / PET / optical fiber substrate by an immersion and pulling method to obtain a sea urchin-shaped Au@Pd nanoarray hydrogen sensor. The plasma resonance peak of Au in the sensor containing perfluorodecanethiol will not change after the hydrogen reaction, and the absorbance at a certain wavelength is less affected when it is selected as a response, and the detection accuracy is higher.

[0045] 3. The hydrogen sensor provided in the present application solves the problem of poor repeatability of the hydrogen sensor formed by self-assembly of nanoparticles while realizing the selective detection of hydrogen by the sensor by spin coating a PMMA polymer layer of a certain thickness.

[0046] 4. The urchin-shaped Au@Pd nanoparticles and hydrogen sensor provided by the present invention solve the shortcomings of high operating temperature, complex sensor manufacturing process and high cost in the prior art, and have the advantages of simple preparation, low response concentration and room temperature detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a transmission electron microscopy test image of the sea urchin-shaped Au@Pd nanomaterial prepared in Example 1.

[0048] Figure 2 The UV absorption spectra of the sensor with and without PFT (perfluorodecanethiol) before and after hydrogen response.

[0049] Figure 3 This is a graph showing the effect of different spin coating speeds on the sensor response time. DETAILED DESCRIPTION

[0050] The present invention will be described in detail below in conjunction with the accompanying drawings.

[0051] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0052] Example 1

[0053] Preparation of Au nanoparticles

[0054] S1, mixing chloroauric acid, hexadecyltrimethylammonium bromide (CTAB), and sodium borohydride and letting stand for 1.5 hours to obtain an Au seed solution;

[0055] The molar ratio of chloroauric acid, hexadecyltrimethylammonium bromide and sodium borohydride is 1:22:2.2.

[0056] S2, adding the Au seed solution prepared in step S1 to an aqueous solution containing CTAB, chloroauric acid, and L-ascorbic acid, shaking and leaving for 12 hours, to obtain Au nanoparticles;

[0057] The molar ratio of Au atoms, CTAB, chloroauric acid, L-ascorbic acid, and water in the Au seed solution is 2:2.2×10 5 : 3×10 3 :1.5×10 4 :1.

[0058] Preparation of sea urchin-like Au@Pd nanomaterials

[0059] Step 1, centrifugally washing Au nanoparticles using a hexadecyltrimethylammonium chloride aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium chloride aqueous solution and mixing them evenly;

[0060] Step 2, controlling the temperature of the mixture obtained in step 1 at 36° C., and keeping the mixture for 15 hours to obtain a sea urchin-shaped Au@Pd nanomaterial;

[0061] The molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium chloride was 1:5:4×10 3 .

[0062] The molar ratio of palladium chloride and L-ascorbic acid added was 2.5:1.

[0063] The sea urchin-shaped Au@Pd nanomaterial prepared in Example 1 was tested by transmission electron microscopy. Figure 1 As stated, Figure 1 It is shown in the figure that the nanomaterial has Au particles as the core, Pd is wrapped around the outside of the core particles, and forms thorn-like protrusions on the surface.

[0064] Preparation of hydrogen sensor

[0065] Take 40ml of the synthesized sea urchin-shaped Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse it in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0066] Example 2

[0067] Preparation of Au nanoparticles

[0068] S1, mixing chloroauric acid, hexadecyltrimethylammonium bromide (CTAB), and sodium borohydride and letting stand for 1.5 hours to obtain an Au seed solution;

[0069] The molar ratio of chloroauric acid, hexadecyltrimethylammonium bromide and sodium borohydride is 1:20:2.5.

[0070] S2, adding the Au seed solution prepared in step S1 to an aqueous solution containing CTAB, chloroauric acid, and L-ascorbic acid, shaking and leaving for 12 hours, to obtain Au nanoparticles;

[0071] The molar ratio of Au atoms, CTAB, chloroauric acid, L-ascorbic acid, and water in the Au seed solution is 1:2.5×10 5 :2.5×10 3 : 2×10 4 :1.

[0072] Preparation of sea urchin-like Au@Pd nanomaterials

[0073] Step 1, centrifugally washing Au nanoparticles using a hexadecyltrimethylammonium chloride aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium chloride aqueous solution and mixing them evenly;

[0074] Step 2, controlling the temperature of the mixture obtained in step 1 at 38° C., and keeping the mixture for 12 hours to obtain a sea urchin-shaped Au@Pd nanomaterial;

[0075] The molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium chloride was 1:8:3.5×10 3 .

[0076] The molar ratio of palladium chloride and L-ascorbic acid added was 3:1.

[0077] Preparation of hydrogen sensor

[0078] Take 40ml of the synthesized sea urchin-shaped Au@Pd nanomaterial, centrifuge and wash for 10min at 11000r / min, and disperse it in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s. You can observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, you can use a clean glass sheet to transfer the nanoparticle film to the glass sheet by the Czochralski method to form an Au@Pd sensor.

[0079] Example 3

[0080] Preparation of Au nanoparticles

[0081] S1, mixing chloroauric acid, hexadecyltrimethylammonium bromide (CTAB), and sodium borohydride and letting stand for 1.5 hours to obtain an Au seed solution;

[0082] The molar ratio of chloroauric acid, hexadecyltrimethylammonium bromide and sodium borohydride is 1:25:2.

[0083] S2, adding the Au seed solution prepared in step S1 to an aqueous solution containing CTAB, chloroauric acid, and L-ascorbic acid, shaking and leaving for 12 hours, to obtain Au nanoparticles;

[0084] The molar ratio of Au atoms, CTAB, chloroauric acid, L-ascorbic acid, and water in the Au seed solution is 3:2×10 5 :3.5×10 3 :1×10 4 :1.

[0085] Preparation of sea urchin-like Au@Pd nanomaterials

[0086] Step 1, centrifugally washing Au nanoparticles using a hexadecyltrimethylammonium chloride aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium chloride aqueous solution and mixing them evenly;

[0087] Step 2, controlling the temperature of the mixture obtained in step 1 at 34° C., and keeping the mixture for 16 hours to obtain a sea urchin-shaped Au@Pd nanomaterial;

[0088] The molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium chloride was 1:1.6:4.5×103 .

[0089] The molar ratio of palladium chloride and L-ascorbic acid added was 2:1.

[0090] Preparation of hydrogen sensor

[0091] Take 40ml of the synthesized sea urchin-shaped Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse it in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0092] Comparative Example 1

[0093] Comparative Example 1 Compared with Example 1, hexadecyltrimethylammonium chloride was not added when preparing the Au@Pd nanomaterial, and the other preparation processes were the same as those of Example 1.

[0094] The Au nanoparticles used in Comparative Example 1 were prepared using the same method as in Example 1.

[0095] Preparation of Au@Pd nanomaterials

[0096] Step 1, mixing Au nanoparticles, palladium chloride and L-ascorbic acid evenly;

[0097] Step 2, controlling the temperature of the mixture obtained in step 1 at 36° C., and keeping the temperature for 15 hours to obtain Au@Pd nanomaterials;

[0098] The molar ratio of Au nanoparticles to palladium chloride is 1:5.

[0099] The molar ratio of palladium chloride and L-ascorbic acid added was 2.5:1.

[0100] Preparation of hydrogen sensor

[0101] Take 40ml of the synthesized Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0102] Comparative Example 2

[0103] Comparative Example 2 Compared with Example 1, hexadecyltrimethylammonium chloride was replaced with hexadecyltrimethylammonium bromide when preparing Au@Pd nanomaterials, and the other preparation processes were the same as those in Example 1.

[0104] The Au nanoparticles used in Comparative Example 2 were prepared using the same method as in Example 1.

[0105] Preparation of Au@Pd nanomaterials

[0106] Step 1, centrifugally washing Au nanoparticles with a hexadecyltrimethylammonium bromide aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium bromide aqueous solution and mixing them evenly;

[0107] Step 2, controlling the temperature of the mixture obtained in step 1 at 36° C., and keeping the temperature for 15 hours to obtain Au@Pd nanomaterials;

[0108] The molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium bromide was 1:5:4×10 3 .

[0109] The molar ratio of palladium chloride and L-ascorbic acid added was 2.5:1.

[0110] Preparation of hydrogen sensor

[0111] Take 40ml of the synthesized Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0112] Comparative Example 3

[0113] Comparative Example 3 Compared with Example 1, the addition ratio of hexadecyltrimethylammonium chloride was changed when preparing Au@Pd nanomaterials, and the other preparation processes were the same as those of Example 1.

[0114] The Au nanoparticles used in Comparative Example 3 were prepared using the same method as in Example 1.

[0115] Preparation of Au@Pd nanomaterials

[0116] Step 1, centrifugally washing Au nanoparticles using a hexadecyltrimethylammonium chloride aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium chloride aqueous solution and mixing them evenly;

[0117] Step 2, controlling the temperature of the mixture obtained in step 1 at 36° C., and keeping the temperature for 15 hours to obtain Au@Pd nanomaterials;

[0118] The molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium chloride was 1:5:2×10 3 .

[0119] The molar ratio of palladium chloride and L-ascorbic acid added was 2.5:1.

[0120] Preparation of hydrogen sensor

[0121] Take 40ml of the synthesized Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0122] Comparative Example 4

[0123] Compared with Example 1, Comparative Example 4 changed the addition ratio of palladium chloride when preparing Au@Pd nanomaterials, and the other preparation processes were the same as those of Example 1.

[0124] The Au nanoparticles used in Comparative Example 4 were prepared using the same method as in Example 1.

[0125] Preparation of Au@Pd nanomaterials

[0126] Step 1, centrifugally washing Au nanoparticles using a hexadecyltrimethylammonium chloride aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium chloride aqueous solution and mixing them evenly;

[0127] Step 2, controlling the temperature of the mixture obtained in step 1 at 36° C., and keeping the temperature for 15 hours to obtain Au@Pd nanomaterials;

[0128] The molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium chloride was 1:1:4×10 3 .

[0129] The molar ratio of palladium chloride and L-ascorbic acid added was 2.5:1.

[0130] Preparation of hydrogen sensor

[0131] Take 40ml of the synthesized Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0132] Comparative Example 5

[0133] Compared with Example 1, Comparative Example 5 changes the addition ratio of palladium chloride when preparing Au@Pd nanomaterials, and the other preparation processes are the same as those of Example 1.

[0134] The Au nanoparticles used in Comparative Example 5 were prepared using the same method as in Example 1.

[0135] Preparation of Au@Pd nanomaterials

[0136] Step 1, centrifugally washing Au nanoparticles using a hexadecyltrimethylammonium chloride aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium chloride aqueous solution and mixing them evenly;

[0137] Step 2, controlling the temperature of the mixture obtained in step 1 at 36° C., and keeping the temperature for 15 hours to obtain Au@Pd nanomaterials;

[0138] The molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium chloride was 1:10:4×10 3 .

[0139] The molar ratio of palladium chloride and L-ascorbic acid added was 2.5:1.

[0140] Preparation of hydrogen sensor

[0141] Take 40ml of the synthesized Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0142] Comparative Example 6

[0143] Compared with Example 1, the reaction temperature was changed when preparing the Au@Pd nanomaterial in Comparative Example 6, and the other preparation processes were the same as those in Example 1.

[0144] The Au nanoparticles used in Comparative Example 6 were prepared using the same method as in Example 1.

[0145] Preparation of Au@Pd nanomaterials

[0146] Step 1, centrifugally washing Au nanoparticles using a hexadecyltrimethylammonium chloride aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium chloride aqueous solution and mixing them evenly;

[0147] Step 2, controlling the temperature of the mixture obtained in step 1 at 30° C., and keeping the temperature for 15 hours to obtain Au@Pd nanomaterials;

[0148] The added molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium chloride is 1:2.5:7.5.

[0149] The molar ratio of palladium chloride and L-ascorbic acid added was 2.5:1.

[0150] Preparation of hydrogen sensor

[0151] Take 40ml of the synthesized Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0152] Comparative Example 7

[0153] Compared with Example 1, the reaction temperature was changed when preparing the Au@Pd nanomaterial in Comparative Example 7, and the other preparation processes were the same as those in Example 1.

[0154] The Au nanoparticles used in Comparative Example 7 were prepared using the same method as in Example 1.

[0155] Preparation of Au@Pd nanomaterials

[0156] Step 1, centrifugally washing Au nanoparticles using a hexadecyltrimethylammonium chloride aqueous solution; then adding the washed Au nanoparticles, palladium chloride, and L-ascorbic acid into the hexadecyltrimethylammonium chloride aqueous solution and mixing them evenly;

[0157] Step 2, controlling the temperature of the mixture obtained in step 1 at 40° C., and keeping the temperature for 15 hours to obtain Au@Pd nanomaterials;

[0158] The added molar ratio of Au nanoparticles, palladium chloride, and hexadecyltrimethylammonium chloride is 1:2.5:7.5.

[0159] The molar ratio of palladium chloride and L-ascorbic acid added was 2.5:1.

[0160] Preparation of hydrogen sensor

[0161] Take 40ml of the synthesized Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse in 8ml water. Then take the washed Au@Pd nanomaterial (7.5ml) and add it to a 25ml beaker, then add 5ml of n-hexane to the beaker to form an oil-water interface, and then add 10ml of anhydrous ethanol to the water phase. After adding, shake the beaker slightly for 3s, and then let it stand for 2s to observe the formation of a nanoparticle film on the interface between n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0162] Test 1

[0163] The sensors prepared in Examples 1-3 and Comparative Examples 1-7 were tested for response time and low detection limit. The test results are shown in Table 1.

[0164] The Ocean Optical USB4000 integrated spectrometer was used to collect the UV absorption spectrum during the sensing process. A cuvette was used as the box body, the prepared sensor was placed in the cuvette, and then the hydrogen tube was placed at the bottom of the cuvette, and hydrogen with a volume concentration of 3% and a volume concentration of 100% were introduced respectively. During the process, the changes in the UV absorption spectrum were recorded in real time, and a △A / t90 graph was drawn, where △A is the absorbance change value, and t90 is the time corresponding to 90% of the maximum absorbance decrease value.

[0165] The test process of low detection limit: The process of hydrogen detection with a volume fraction of 0.1% is as follows: 1. Place the prepared sensor in a cuvette, and then place the cuvette in the USB 4000. 2. The gas tube of the gas cylinder containing 0.1% hydrogen goes deep into the bottom of the cuvette. 3. Open the gas valve and start recording the real-time changes of the sensor's UV-visible absorption spectrum until the UV-visible absorption spectrum stabilizes. 4. Take out the hydrogen tube during desorption, and keep recording the UV-visible absorption spectrum in real time until it stabilizes. 5. Finally, judge the hydrogen concentration by the change of absorbance at a certain wavelength selected.

[0166] Table 1

[0167]

[0168] Example 4

[0169] Example 4 uses the sea urchin-shaped Au@Pd nanomaterial prepared in Example 1.

[0170] Preparation of hydrogen sensor

[0171] Take 40ml of the synthesized sea urchin-shaped Au@Pd nanomaterial, centrifuge and wash for 10min at 11000r / min, and disperse it in 8ml water. Then take the washed Au@Pd nanoparticles (7.5ml) and add them to a 25ml beaker, then add perfluorodecanethiol solution (10mM, 15ml, solvent is n-hexane: anhydrous ethanol = 1:2), shake the beaker slightly for 3s after adding, and then let it stand for 2s to observe the formation of nanoparticle film on the interface of n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0172] Example 5

[0173] Example 5 uses the sea urchin-shaped Au@Pd nanomaterial prepared in Example 2.

[0174] Preparation of hydrogen sensor

[0175] Take 40ml of the synthesized sea urchin-shaped Au@Pd nanomaterial, centrifuge and wash at 11000r / min for 10min, and disperse in 8ml water. Then take the washed Au@Pd nanoparticles (7.5ml) and add them to a 25ml beaker, then add perfluorodecanethiol solution (8mM, 18ml, solvent is n-hexane: anhydrous ethanol = 1:1.5), shake the beaker slightly for 3s after adding, and then let it stand for 2s to observe the formation of nanoparticle film on the interface of n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0176] test

[0177] The response time of the sensor prepared in Example 4-5 and whether the plasma resonance peak of Au changes after the hydrogen reaction were tested. The test results are shown in Table 2.

[0178] The Ocean Optical USB4000 integrated spectrometer was used to collect the UV absorption spectrum during the sensing process. A cuvette was used as the box body, the prepared sensor was placed in the cuvette, and then the hydrogen tube was placed at the bottom of the cuvette. The changes in the UV absorption spectrum were recorded in real time during the process of passing 3% hydrogen.

[0179] Table 2

[0180]

[0181]

[0182] The presence of perfluorodecanethiol will increase the response time of the sensor. This is because the presence of the thiol group will hinder the reaction between hydrogen and Pd to a certain extent, so it will increase the response time. However, for sensors without perfluorodecanethiol, the plasma resonance peak of Au changes after the hydrogen reaction, which will have a huge impact when we choose the absorbance of a certain wavelength as the response. Although the presence of perfluorodecanethiol will increase the response time, it can be used as a preferred case because the plasma resonance peak of Au will not change after the hydrogen reaction. Figure 2 As shown, the ultraviolet absorption spectra of the sensors prepared in Example 1 and Example 4 with and without PFT (perfluorodecanethiol) before and after hydrogen response.

[0183] Embodiment 6-15

[0184] Examples 6-15 use the sea urchin-shaped Au@Pd nanomaterial prepared in Example 1.

[0185] Preparation of hydrogen sensor

[0186] Take 40ml of the synthesized sea urchin-shaped Au@Pd nanomaterial, centrifuge and wash for 10min at 11000r / min, and disperse it in 8ml water. Then take the washed Au@Pd nanoparticles (7.5ml) and add them to a 25ml beaker, then add perfluorodecanethiol solution (10mM, 15ml, solvent is n-hexane: anhydrous ethanol = 1:2), shake the beaker slightly for 3s after adding, and then let it stand for 2s to observe the formation of nanoparticle film on the interface of n-hexane and water. After the n-hexane evaporates completely, the nanoparticle film can be transferred to the glass slide by the Czochralski method using a clean glass slide to form an Au@Pd sensor.

[0187] Example 6-15 Take the prepared Au@Pd sensor above, place it on a spin coater, and then spin coat 4wt% PMMA at a spin coating speed of 500, 1000, 1500, 2000, 3000, 4000, 5000, 6000, and 7000 r / min, respectively. The spin coating time is 30 s. After the spin coating is completed, place the sensor on a heating plate and heat it at 50°C for 10 min to form a PMMA-Au@Pd hydrogen sensor.

[0188] The Ocean Optical USB4000 integrated spectrometer was used to collect the UV absorption spectrum during the sensing process. A cuvette was used as the box body, the prepared sensor was placed in the cuvette, and then the hydrogen tube was placed at the bottom of the cuvette. The changes in the UV absorption spectrum were recorded in real time during the process of passing 3% hydrogen. A Time / Spin-coating Speed ​​graph was drawn, where Time is the time when the absorbance drops to the maximum value, and Spin-coating Speed ​​is the spin coating speed during spin coating.

[0189] The difference parameters in the process of preparing the sea urchin-shaped Au@Pd sensor in Example 6-15 are shown in the following table, and the sensor performance is tested. The results are shown in the following table. The specific embodiment parameters are shown in Table 3 below.

[0190] Table 3

[0191]

[0192] Different spin coating speeds have a great influence on the performance of the sensor. The response time of the sensor is inversely proportional to the spin coating speed (except when the spin coating speed is 0). This is because the thicker PMMA layer causes a longer diffusion time of hydrogen in it, which increases the overall response time of the sensor. When the PMMA layer becomes thinner, especially at a spin coating speed of 7000r / min, the response time of the sensor will be shortened. This is because the PMMA layer itself has the function of reducing the activation energy of the reaction between Pd and hydrogen. Only when the inhibition brought by the PMMA thickness cannot offset the shortening brought by it can the performance of PMMA in reducing the activation energy be shown. The sensor cycle performance is significantly improved at a spin coating speed of 500-6000r / min, but when the spin coating speed continues to increase, the sensor cycle performance deteriorates rapidly. This is because the presence of PMMA inhibits the phase change of the Pd layer during the reaction with hydrogen, thereby improving the cycle performance of the sensor. However, when PMMA is thinner, it cannot better inhibit the phase change of Pd, so the sensor cyclability deteriorates. Specifically, Figure 3 As shown, the effect of different spin coating speeds on the sensor response time.

[0193] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a sea urchin-shaped Au@Pd nanomaterial, characterized in that: The following steps are involved: Step 1, adding Au nanoparticles, palladium chloride and L-ascorbic acid into a hexadecyltrimethylammonium chloride aqueous solution and mixing evenly; Step 2, controlling the temperature of the mixture obtained in step 1 to 34-38° C., and performing a heat-retention reaction to obtain a sea urchin-shaped Au@Pd nanomaterial; The molar amount of hexadecyltrimethylammonium chloride added is 3.5×10 of the molar amount of Au nanoparticles added. 3 times or more; The molar ratio of Au nanoparticles to palladium chloride is 1:1.6-8.

2. The method for preparing the sea urchin-shaped Au@Pd nanomaterial according to claim 1, characterized in that: The molar ratio of Au nanoparticles to hexadecyltrimethylammonium chloride is 1:3.5×10 3 ~4.5×10 3 .

3. The method for preparing the sea urchin-shaped Au@Pd nanomaterial according to claim 1, characterized in that: The molar ratio of palladium chloride and L-ascorbic acid added is 2 to 3:

1.

4. The method for preparing the sea urchin-shaped Au@Pd nanomaterial according to claim 1, characterized in that: Before step 1, the Au nanoparticles are washed by centrifugation using a hexadecyltrimethylammonium chloride aqueous solution.

5. The method for preparing the sea urchin-shaped Au@Pd nanomaterial according to claim 1, characterized in that: Au nanoparticles were prepared by the following method: S1, mixing chloroauric acid, hexadecyltrimethylammonium bromide and sodium borohydride and letting it stand to obtain an Au seed solution; S2. Add the Au seed solution prepared in step S1 to an aqueous solution containing CTAB, chloroauric acid, and L-ascorbic acid, shake and allow to react, and centrifuge to remove the supernatant to obtain Au nanoparticles.

6. The method for preparing the sea urchin-shaped Au@Pd nanomaterial according to claim 1, characterized in that: In the step 2, the temperature of the mixture obtained in the step 1 is controlled at 35-36°C.

7. The method for preparing the sea urchin-shaped Au@Pd nanomaterial according to any one of claims 1 to 6, characterized in that: In step 2, the heat preservation reaction time is 12 to 16 hours.

8. A sea urchin-shaped Au@Pd nanomaterial prepared by the method for preparing a sea urchin-shaped Au@Pd nanomaterial according to any one of claims 1 to 7.

9. A hydrogen sensor, characterized in that: It is prepared using the sea urchin-shaped Au@Pd nanomaterial as described in claim 8.

10. A method for preparing a hydrogen sensor, characterized in that: The following steps are involved: A1. Add the sea urchin-shaped Au@Pd nanomaterial as claimed in claim 8 to a perfluorodecanethiol solution, mix, and allow to stand; wherein the perfluorodecanethiol solution uses a mixture of ethanol and n-hexane as a solvent; A2. After the n-hexane evaporates, Au@Pd nanoparticles are loaded onto the substrate using a glass slide to obtain a hydrogen sensor.

Citation Information

Cited By

  • Preparation method of optical fiber LSPR (Localized Surface Plasmon Resonance) sensor based on gold nanocrystal modification

    CN119574508A